EN 10088-1 Grade X2CrNi19-11 strain-hardened (+C700)

Want to keep this datasheet? Save it now in your required format

Description

Material X2CrNi19-11a modifikation of 1.4301 is comparable to X 2CrNi 19 11 acc. to DIN 17440 : 1985-07. The steel shows owing to the lowered C-content resistance to intercrystalline corrosion both in delivery and sensitized condition. Application in chemical apparatus engineering and in pharmaceutical industry, especially when high wall thickness and simultaneous suitability for mirror finishing are requested in atomic reactor technology, for parts in food industry which are exposed to organic or fruit acids, in oil, soap and synthetic fibre industry. Generally resistant up to pH-value 4,5 in aggressive agents.

Related Standards

Equivalent Materials

This material data has been provided by WIAM.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValue

Density

20.0 °C

7.9 - 7.92 g/cm³

Show Material materials with Density of 7.9 - 7.92 g/cm³

Mechanical

PropertyTemperatureValue

Elastic modulus

-269.0 °C

201.3 GPa

Show Material materials with Elastic modulus of 201.3 GPa

-195.0 °C

205.1 GPa

Show Material materials with Elastic modulus of 205.1 GPa

-100.0 °C

206 GPa

Show Material materials with Elastic modulus of 206 GPa

20.0 °C

196 - 200 GPa

Show Material materials with Elastic modulus of 196 - 200 GPa

27.0 °C

190.2 GPa

Show Material materials with Elastic modulus of 190.2 GPa

100.0 °C

190 - 194 GPa

Show Material materials with Elastic modulus of 190 - 194 GPa

200.0 °C

182 - 186 GPa

Show Material materials with Elastic modulus of 182 - 186 GPa

300.0 °C

174 - 179 GPa

Show Material materials with Elastic modulus of 174 - 179 GPa

400.0 °C

166 - 172 GPa

Show Material materials with Elastic modulus of 166 - 172 GPa

500.0 °C

158 - 165 GPa

Show Material materials with Elastic modulus of 158 - 165 GPa

600.0 °C

150 GPa

Show Material materials with Elastic modulus of 150 GPa

700.0 °C

142 GPa

Show Material materials with Elastic modulus of 142 GPa

800.0 °C

134 GPa

Show Material materials with Elastic modulus of 134 GPa

Elongation

20.0 °C

20 %

Show Material materials with Elongation of 20 %

Poisson's ratio

-269.0 °C

0.31 [-]

Show Material materials with Poisson's ratio of 0.31 [-]

-195.0 °C

0.29 [-]

Show Material materials with Poisson's ratio of 0.29 [-]

20.0 °C

0.29 [-]

Show Material materials with Poisson's ratio of 0.29 [-]

27.0 °C

0.27 [-]

Show Material materials with Poisson's ratio of 0.27 [-]

Unlock all property charts

Shear modulus

20.0 °C

75.7 GPa

Show Material materials with Shear modulus of 75.7 GPa

Tensile strength

20.0 °C

700 - 900 MPa

Show Material materials with Tensile strength of 700 - 900 MPa

Yield strength Rp0.2

20.0 °C

350 MPa

Show Material materials with Yield strength Rp0.2 of 350 MPa

Thermal

PropertyTemperatureValueComment

Coefficient of thermal expansion

-100.0 °C

1.49E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.49E-5 1/K

20.0 °C

1.61E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.61E-5 1/K

100.0 °C

1.6E-5 - 1.67E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.6E-5 - 1.67E-5 1/K

200.0 °C

1.65E-5 - 1.72E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.65E-5 - 1.72E-5 1/K

300.0 °C

1.7E-5 - 1.77E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.7E-5 - 1.77E-5 1/K

400.0 °C

1.75E-5 - 1.81E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.75E-5 - 1.81E-5 1/K

500.0 °C

1.8E-5 - 1.84E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.8E-5 - 1.84E-5 1/K

600.0 °C

1.88E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.88E-5 1/K

700.0 °C

1.91E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.91E-5 1/K

800.0 °C

1.94E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.94E-5 1/K

Unlock all property charts

Melting point

1230 - 1480 °C

Show Material materials with Melting point of 1230 - 1480 °C

Typical for Austenitic Stainless Steel

Specific heat capacity

-100.0 °C

440 J/(kg·K)

Show Material materials with Specific heat capacity of 440 J/(kg·K)

20.0 °C

472 - 500 J/(kg·K)

Show Material materials with Specific heat capacity of 472 - 500 J/(kg·K)

100.0 °C

487 J/(kg·K)

Show Material materials with Specific heat capacity of 487 J/(kg·K)

200.0 °C

503 J/(kg·K)

Show Material materials with Specific heat capacity of 503 J/(kg·K)

300.0 °C

512 J/(kg·K)

Show Material materials with Specific heat capacity of 512 J/(kg·K)

400.0 °C

520 J/(kg·K)

Show Material materials with Specific heat capacity of 520 J/(kg·K)

500.0 °C

530 J/(kg·K)

Show Material materials with Specific heat capacity of 530 J/(kg·K)

600.0 °C

541 J/(kg·K)

Show Material materials with Specific heat capacity of 541 J/(kg·K)

700.0 °C

551 J/(kg·K)

Show Material materials with Specific heat capacity of 551 J/(kg·K)

800.0 °C

559 J/(kg·K)

Show Material materials with Specific heat capacity of 559 J/(kg·K)

Unlock all property charts

Thermal conductivity

20.0 °C

13.9 - 15 W/(m·K)

Show Material materials with Thermal conductivity of 13.9 - 15 W/(m·K)

100.0 °C

15.4 W/(m·K)

Show Material materials with Thermal conductivity of 15.4 W/(m·K)

200.0 °C

17.2 W/(m·K)

Show Material materials with Thermal conductivity of 17.2 W/(m·K)

300.0 °C

18.7 W/(m·K)

Show Material materials with Thermal conductivity of 18.7 W/(m·K)

400.0 °C

20.2 W/(m·K)

Show Material materials with Thermal conductivity of 20.2 W/(m·K)

500.0 °C

21.6 W/(m·K)

Show Material materials with Thermal conductivity of 21.6 W/(m·K)

600.0 °C

23 W/(m·K)

Show Material materials with Thermal conductivity of 23 W/(m·K)

700.0 °C

24.4 W/(m·K)

Show Material materials with Thermal conductivity of 24.4 W/(m·K)

800.0 °C

25.8 W/(m·K)

Show Material materials with Thermal conductivity of 25.8 W/(m·K)

Unlock all property charts

Thermal diffusivity

20.0 °C

3.7 mm²/s

Show Material materials with Thermal diffusivity of 3.7 mm²/s

100.0 °C

3.9 mm²/s

Show Material materials with Thermal diffusivity of 3.9 mm²/s

200.0 °C

4.2 mm²/s

Show Material materials with Thermal diffusivity of 4.2 mm²/s

300.0 °C

4.5 mm²/s

Show Material materials with Thermal diffusivity of 4.5 mm²/s

400.0 °C

4.7 mm²/s

Show Material materials with Thermal diffusivity of 4.7 mm²/s

500.0 °C

4.8 mm²/s

Show Material materials with Thermal diffusivity of 4.8 mm²/s

600.0 °C

5 mm²/s

Show Material materials with Thermal diffusivity of 5 mm²/s

700.0 °C

5.3 mm²/s

Show Material materials with Thermal diffusivity of 5.3 mm²/s

800.0 °C

5.6 mm²/s

Show Material materials with Thermal diffusivity of 5.6 mm²/s

Unlock all property charts

Electrical

PropertyTemperatureValue

Electrical resistivity

20.0 °C

7.3E-7 - 7.35E-7 Ω·m

Show Material materials with Electrical resistivity of 7.3E-7 - 7.35E-7 Ω·m

100.0 °C

8E-7 Ω·m

Show Material materials with Electrical resistivity of 8E-7 Ω·m

200.0 °C

8.68E-7 Ω·m

Show Material materials with Electrical resistivity of 8.68E-7 Ω·m

300.0 °C

9.33E-7 Ω·m

Show Material materials with Electrical resistivity of 9.33E-7 Ω·m

400.0 °C

9.89E-7 Ω·m

Show Material materials with Electrical resistivity of 9.89E-7 Ω·m

500.0 °C

1.04E-6 Ω·m

Show Material materials with Electrical resistivity of 1.04E-6 Ω·m

600.0 °C

1.08E-6 Ω·m

Show Material materials with Electrical resistivity of 1.08E-6 Ω·m

700.0 °C

1.12E-6 Ω·m

Show Material materials with Electrical resistivity of 1.12E-6 Ω·m

800.0 °C

1.15E-6 Ω·m

Show Material materials with Electrical resistivity of 1.15E-6 Ω·m

Unlock all property charts

Chemical properties

PropertyValue

Carbon

0.03 %

Show Material materials with Carbon of 0.03 %

Chromium

18 - 20 %

Show Material materials with Chromium of 18 - 20 %

Manganese

2 %

Show Material materials with Manganese of 2 %

Nickel

10 - 12 %

Show Material materials with Nickel of 10 - 12 %

Nitrogen

0.11 %

Show Material materials with Nitrogen of 0.11 %

Phosphorus

0.05 %

Show Material materials with Phosphorus of 0.05 %

Silicon

1 %

Show Material materials with Silicon of 1 %

Sulfur

0.015 %

Show Material materials with Sulfur of 0.015 %