EN 10088-1 Grade X2CrNiMoN17-13-5 solution annealed (+AT)

Want to keep this datasheet? Save it now in your required format

Description

Material X 2 CrNiMoN 17 13 5 (now: X2CrNiMoN17-13-5), material number 1.4539, is applicated acc. to VdTÜV-Wbl 405 : 2000-12 for pressure vessels acc. to TRB 100 and AD-data sheets W 2 and W 10 from -196 to 400 °C. and for pressure gas tanks as per TRG 201 and TRG 203 from -196 to 400 °C. Further application in nuclear power engineering as far as nuclear rules or object-related specifications permit use from -196 to 400 °C. The austenitic rolled and forged steel is cold and warm formable. Its welding suitability is allowing for general accepted engineering rules examined for the following welding methods: arc hand welding, tungsten inert-gas welding, submerged welding and plasma welding. A pre-heating is not necessary, a heat after treatment (solution annealing with subsequent quenching) is required only in certain cases (special corrosion load). Steel X2CrNiMoN17-13-5 is comparable to X 2 CrNiMoN 17 13 5 acc. to DIN 17440 : 1985-07 (invalid). The material shows high pitting and crevice corrosion resistance (more favorable properties than 1.4436) as well as stress corrosion resistance, highest general resistance in many organic acids with high concentration and temperature, e.g. in nonoxidizing acids and chloride containing media (seawater, hypochloride base), also in inorganic and mixed acids as well as resistance to intercrystalline corrosion also in sensitized condition. Application in reactor industry, offshore technology, chemical industry.

Related Standards

Equivalent Materials

This material data has been provided by WIAM.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValue

Density

20.0 °C

8 - 8.01 g/cm³

Show Material materials with Density of 8 - 8.01 g/cm³

Mechanical

PropertyTemperatureValue

Elastic modulus

-100.0 °C

206 GPa

Show Material materials with Elastic modulus of 206 GPa

20.0 °C

196 - 200 GPa

Show Material materials with Elastic modulus of 196 - 200 GPa

100.0 °C

190 - 194 GPa

Show Material materials with Elastic modulus of 190 - 194 GPa

200.0 °C

182 - 186 GPa

Show Material materials with Elastic modulus of 182 - 186 GPa

300.0 °C

174 - 179 GPa

Show Material materials with Elastic modulus of 174 - 179 GPa

400.0 °C

166 - 172 GPa

Show Material materials with Elastic modulus of 166 - 172 GPa

500.0 °C

158 - 165 GPa

Show Material materials with Elastic modulus of 158 - 165 GPa

600.0 °C

150 GPa

Show Material materials with Elastic modulus of 150 GPa

700.0 °C

142 GPa

Show Material materials with Elastic modulus of 142 GPa

800.0 °C

134 GPa

Show Material materials with Elastic modulus of 134 GPa

Elongation

20.0 °C

35 %

Show Material materials with Elongation of 35 %

Elongation A80, transverse

20.0 °C

35 - 40 %

Show Material materials with Elongation A80, transverse of 35 - 40 %

Elongation, transverse

20.0 °C

30 - 40 %

Show Material materials with Elongation, transverse of 30 - 40 %

Hardness, Brinell

20.0 °C

250 [-]

Show Material materials with Hardness, Brinell of 250 [-]

Hardness, Brinell, trans

20.0 °C

250 [-]

Show Material materials with Hardness, Brinell, trans of 250 [-]

Poisson's ratio

20.0 °C

0.28 [-]

Show Material materials with Poisson's ratio of 0.28 [-]

Shear modulus

20.0 °C

77.3 GPa

Show Material materials with Shear modulus of 77.3 GPa

Tensile strength

20.0 °C

580 - 800 MPa

Show Material materials with Tensile strength of 580 - 800 MPa

Tensile strength, transverse

20.0 °C

580 - 800 MPa

Show Material materials with Tensile strength, transverse of 580 - 800 MPa

Yield strength Rp0.2

20.0 °C

280 MPa

Show Material materials with Yield strength Rp0.2 of 280 MPa

100.0 °C

225 MPa

Show Material materials with Yield strength Rp0.2 of 225 MPa

150.0 °C

200 MPa

Show Material materials with Yield strength Rp0.2 of 200 MPa

200.0 °C

185 MPa

Show Material materials with Yield strength Rp0.2 of 185 MPa

250.0 °C

175 MPa

Show Material materials with Yield strength Rp0.2 of 175 MPa

300.0 °C

165 MPa

Show Material materials with Yield strength Rp0.2 of 165 MPa

350.0 °C

155 MPa

Show Material materials with Yield strength Rp0.2 of 155 MPa

400.0 °C

150 MPa

Show Material materials with Yield strength Rp0.2 of 150 MPa

Unlock all property charts

Yield strength Rp0.2, transverse

20.0 °C

270 - 290 MPa

Show Material materials with Yield strength Rp0.2, transverse of 270 - 290 MPa

Yield strength Rp1.0

20.0 °C

315 MPa

Show Material materials with Yield strength Rp1.0 of 315 MPa

100.0 °C

255 MPa

Show Material materials with Yield strength Rp1.0 of 255 MPa

150.0 °C

230 MPa

Show Material materials with Yield strength Rp1.0 of 230 MPa

200.0 °C

210 MPa

Show Material materials with Yield strength Rp1.0 of 210 MPa

250.0 °C

200 MPa

Show Material materials with Yield strength Rp1.0 of 200 MPa

300.0 °C

190 MPa

Show Material materials with Yield strength Rp1.0 of 190 MPa

350.0 °C

180 MPa

Show Material materials with Yield strength Rp1.0 of 180 MPa

400.0 °C

175 MPa

Show Material materials with Yield strength Rp1.0 of 175 MPa

Unlock all property charts

Yield strength Rp1.0, transverse

20.0 °C

310 - 320 MPa

Show Material materials with Yield strength Rp1.0, transverse of 310 - 320 MPa

Thermal

PropertyTemperatureValueComment

Coefficient of thermal expansion

-100.0 °C

1.49E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.49E-5 1/K

20.0 °C

1.61E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.61E-5 1/K

100.0 °C

1.6E-5 - 1.67E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.6E-5 - 1.67E-5 1/K

200.0 °C

1.65E-5 - 1.72E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.65E-5 - 1.72E-5 1/K

300.0 °C

1.7E-5 - 1.77E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.7E-5 - 1.77E-5 1/K

400.0 °C

1.75E-5 - 1.81E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.75E-5 - 1.81E-5 1/K

500.0 °C

1.8E-5 - 1.84E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.8E-5 - 1.84E-5 1/K

600.0 °C

1.88E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.88E-5 1/K

700.0 °C

1.91E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.91E-5 1/K

800.0 °C

1.94E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.94E-5 1/K

900.0 °C

1.97E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.97E-5 1/K

1000.0 °C

2E-5 1/K

Show Material materials with Coefficient of thermal expansion of 2E-5 1/K

Unlock all property charts

Max service temperature, long

-196 - 400 °C

Show Material materials with Max service temperature, long of -196 - 400 °C

Melting point

1230 - 1480 °C

Show Material materials with Melting point of 1230 - 1480 °C

Typical for Austenitic Stainless Steel

Specific heat capacity

-100.0 °C

440 J/(kg·K)

Show Material materials with Specific heat capacity of 440 J/(kg·K)

20.0 °C

472 - 500 J/(kg·K)

Show Material materials with Specific heat capacity of 472 - 500 J/(kg·K)

100.0 °C

487 J/(kg·K)

Show Material materials with Specific heat capacity of 487 J/(kg·K)

200.0 °C

503 J/(kg·K)

Show Material materials with Specific heat capacity of 503 J/(kg·K)

300.0 °C

512 J/(kg·K)

Show Material materials with Specific heat capacity of 512 J/(kg·K)

400.0 °C

520 J/(kg·K)

Show Material materials with Specific heat capacity of 520 J/(kg·K)

500.0 °C

530 J/(kg·K)

Show Material materials with Specific heat capacity of 530 J/(kg·K)

600.0 °C

541 J/(kg·K)

Show Material materials with Specific heat capacity of 541 J/(kg·K)

700.0 °C

551 J/(kg·K)

Show Material materials with Specific heat capacity of 551 J/(kg·K)

800.0 °C

559 J/(kg·K)

Show Material materials with Specific heat capacity of 559 J/(kg·K)

900.0 °C

565 J/(kg·K)

Show Material materials with Specific heat capacity of 565 J/(kg·K)

1000.0 °C

571 J/(kg·K)

Show Material materials with Specific heat capacity of 571 J/(kg·K)

Unlock all property charts

Thermal conductivity

20.0 °C

13.5 - 14 W/(m·K)

Show Material materials with Thermal conductivity of 13.5 - 14 W/(m·K)

100.0 °C

14.9 W/(m·K)

Show Material materials with Thermal conductivity of 14.9 W/(m·K)

200.0 °C

16.7 W/(m·K)

Show Material materials with Thermal conductivity of 16.7 W/(m·K)

300.0 °C

18.3 W/(m·K)

Show Material materials with Thermal conductivity of 18.3 W/(m·K)

400.0 °C

19.8 W/(m·K)

Show Material materials with Thermal conductivity of 19.8 W/(m·K)

500.0 °C

21.3 W/(m·K)

Show Material materials with Thermal conductivity of 21.3 W/(m·K)

600.0 °C

22.7 W/(m·K)

Show Material materials with Thermal conductivity of 22.7 W/(m·K)

700.0 °C

24.2 W/(m·K)

Show Material materials with Thermal conductivity of 24.2 W/(m·K)

800.0 °C

25.6 W/(m·K)

Show Material materials with Thermal conductivity of 25.6 W/(m·K)

Unlock all property charts

Thermal diffusivity

20.0 °C

3.6 mm²/s

Show Material materials with Thermal diffusivity of 3.6 mm²/s

100.0 °C

3.7 mm²/s

Show Material materials with Thermal diffusivity of 3.7 mm²/s

200.0 °C

4 mm²/s

Show Material materials with Thermal diffusivity of 4 mm²/s

300.0 °C

4.4 mm²/s

Show Material materials with Thermal diffusivity of 4.4 mm²/s

400.0 °C

4.6 mm²/s

Show Material materials with Thermal diffusivity of 4.6 mm²/s

500.0 °C

4.7 mm²/s

Show Material materials with Thermal diffusivity of 4.7 mm²/s

600.0 °C

4.9 mm²/s

Show Material materials with Thermal diffusivity of 4.9 mm²/s

700.0 °C

5.2 mm²/s

Show Material materials with Thermal diffusivity of 5.2 mm²/s

800.0 °C

5.5 mm²/s

Show Material materials with Thermal diffusivity of 5.5 mm²/s

Unlock all property charts

Electrical

PropertyTemperatureValue

Electrical resistivity

20.0 °C

7.75E-7 - 8.5E-7 Ω·m

Show Material materials with Electrical resistivity of 7.75E-7 - 8.5E-7 Ω·m

100.0 °C

8.42E-7 Ω·m

Show Material materials with Electrical resistivity of 8.42E-7 Ω·m

200.0 °C

9.04E-7 Ω·m

Show Material materials with Electrical resistivity of 9.04E-7 Ω·m

300.0 °C

9.62E-7 Ω·m

Show Material materials with Electrical resistivity of 9.62E-7 Ω·m

400.0 °C

1.01E-6 Ω·m

Show Material materials with Electrical resistivity of 1.01E-6 Ω·m

500.0 °C

1.06E-6 Ω·m

Show Material materials with Electrical resistivity of 1.06E-6 Ω·m

600.0 °C

1.1E-6 Ω·m

Show Material materials with Electrical resistivity of 1.1E-6 Ω·m

700.0 °C

1.13E-6 Ω·m

Show Material materials with Electrical resistivity of 1.13E-6 Ω·m

800.0 °C

1.16E-6 Ω·m

Show Material materials with Electrical resistivity of 1.16E-6 Ω·m

Unlock all property charts

Chemical properties

PropertyValue

Carbon

0.03 %

Show Material materials with Carbon of 0.03 %

Chromium

16.5 - 18.5 %

Show Material materials with Chromium of 16.5 - 18.5 %

Manganese

2 %

Show Material materials with Manganese of 2 %

Molybdenum

4 - 5 %

Show Material materials with Molybdenum of 4 - 5 %

Nickel

12.5 - 14.5 %

Show Material materials with Nickel of 12.5 - 14.5 %

Nitrogen

0.12 - 0.22 %

Show Material materials with Nitrogen of 0.12 - 0.22 %

Phosphorus

0.05 %

Show Material materials with Phosphorus of 0.05 %

Silicon

1 %

Show Material materials with Silicon of 1 %

Sulfur

0.015 %