EN 10088-1 Grade X1CrNiMoCuN25-25-5 solution annealed (+AT)

Want to keep this datasheet? Save it now in your required format

Description

The austenitic material X1CrNiMoCuN25-25-5 is used in solution annealed condition in the form of warm rolled sheet, rods, wire rods and profiles. It is resistant to intercrystalline corrosion also in sensitized condition.

Related Standards

Equivalent Materials

This material data has been provided by WIAM.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValue

Density

20.0 °C

8.1 g/cm³

Show Material materials with Density of 8.1 g/cm³

Mechanical

PropertyTemperatureValueComment

Elastic modulus

20.0 °C

195 GPa

Show Material materials with Elastic modulus of 195 GPa

100.0 °C

190 GPa

Show Material materials with Elastic modulus of 190 GPa

200.0 °C

182 GPa

Show Material materials with Elastic modulus of 182 GPa

300.0 °C

174 GPa

Show Material materials with Elastic modulus of 174 GPa

400.0 °C

166 GPa

Show Material materials with Elastic modulus of 166 GPa

500.0 °C

158 GPa

Show Material materials with Elastic modulus of 158 GPa

Elongation

20.0 °C

35 %

Show Material materials with Elongation of 35 %

Elongation A80, transverse

20.0 °C

40 %

Show Material materials with Elongation A80, transverse of 40 %

Elongation, transverse

20.0 °C

30 - 40 %

Show Material materials with Elongation, transverse of 30 - 40 %

Hardness, Brinell

20.0 °C

250 [-]

Show Material materials with Hardness, Brinell of 250 [-]

Hardness, Brinell, trans

20.0 °C

250 [-]

Show Material materials with Hardness, Brinell, trans of 250 [-]

Poisson's ratio

23.0 °C

0.3 [-]

Show Material materials with Poisson's ratio of 0.3 [-]

Typical for Austenitic Stainless Steel

Shear modulus

23.0 °C

77 GPa

Show Material materials with Shear modulus of 77 GPa

Typical for Austenitic Stainless Steel

Tensile strength

20.0 °C

600 - 800 MPa

Show Material materials with Tensile strength of 600 - 800 MPa

Tensile strength, transverse

20.0 °C

600 - 800 MPa

Show Material materials with Tensile strength, transverse of 600 - 800 MPa

Yield strength Rp0.2

20.0 °C

300 MPa

Show Material materials with Yield strength Rp0.2 of 300 MPa

100.0 °C

240 MPa

Show Material materials with Yield strength Rp0.2 of 240 MPa

150.0 °C

220 MPa

Show Material materials with Yield strength Rp0.2 of 220 MPa

200.0 °C

200 MPa

Show Material materials with Yield strength Rp0.2 of 200 MPa

250.0 °C

190 MPa

Show Material materials with Yield strength Rp0.2 of 190 MPa

300.0 °C

180 MPa

Show Material materials with Yield strength Rp0.2 of 180 MPa

350.0 °C

175 MPa

Show Material materials with Yield strength Rp0.2 of 175 MPa

400.0 °C

170 MPa

Show Material materials with Yield strength Rp0.2 of 170 MPa

Unlock all property charts

Yield strength Rp0.2, transverse

20.0 °C

290 - 300 MPa

Show Material materials with Yield strength Rp0.2, transverse of 290 - 300 MPa

Yield strength Rp1.0

20.0 °C

340 MPa

Show Material materials with Yield strength Rp1.0 of 340 MPa

100.0 °C

270 MPa

Show Material materials with Yield strength Rp1.0 of 270 MPa

150.0 °C

250 MPa

Show Material materials with Yield strength Rp1.0 of 250 MPa

200.0 °C

230 MPa

Show Material materials with Yield strength Rp1.0 of 230 MPa

250.0 °C

220 MPa

Show Material materials with Yield strength Rp1.0 of 220 MPa

300.0 °C

210 MPa

Show Material materials with Yield strength Rp1.0 of 210 MPa

350.0 °C

205 MPa

Show Material materials with Yield strength Rp1.0 of 205 MPa

400.0 °C

200 MPa

Show Material materials with Yield strength Rp1.0 of 200 MPa

Unlock all property charts

Yield strength Rp1.0, transverse

20.0 °C

330 - 340 MPa

Show Material materials with Yield strength Rp1.0, transverse of 330 - 340 MPa

Thermal

PropertyTemperatureValueComment

Coefficient of thermal expansion

100.0 °C

1.5E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.5E-5 1/K

300.0 °C

1.65E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.65E-5 1/K

Unlock all property charts

Melting point

1230 - 1480 °C

Show Material materials with Melting point of 1230 - 1480 °C

Typical for Austenitic Stainless Steel

Specific heat capacity

20.0 °C

500 J/(kg·K)

Show Material materials with Specific heat capacity of 500 J/(kg·K)

Thermal conductivity

20.0 °C

14 W/(m·K)

Show Material materials with Thermal conductivity of 14 W/(m·K)

Electrical

PropertyTemperatureValue

Electrical resistivity

20.0 °C

8.5E-7 Ω·m

Show Material materials with Electrical resistivity of 8.5E-7 Ω·m

Chemical properties

PropertyValue

Carbon

0.02 %

Show Material materials with Carbon of 0.02 %

Chromium

24 - 26 %

Show Material materials with Chromium of 24 - 26 %

Copper

1 - 2 %

Show Material materials with Copper of 1 - 2 %

Manganese

2 %

Show Material materials with Manganese of 2 %

Molybdenum

4.7 - 5.7 %

Show Material materials with Molybdenum of 4.7 - 5.7 %

Nickel

24 - 27 %

Show Material materials with Nickel of 24 - 27 %

Nitrogen

0.17 - 0.25 %

Show Material materials with Nitrogen of 0.17 - 0.25 %

Phosphorus

0.03 %

Show Material materials with Phosphorus of 0.03 %

Silicon

0.7 %

Show Material materials with Silicon of 0.7 %

Sulfur

0.01 %

Show Material materials with Sulfur of 0.01 %