General
Property | Temperature | Value |
---|---|---|
Density | 20.0 °C | 7.85 g/cm³ Show Material materials with Density of 7.85 g/cm³ |
Mechanical
Property | Temperature | Value | Comment |
---|---|---|---|
Elastic modulus | 20.0 °C | 210 GPa Show Material materials with Elastic modulus of 210 GPa | |
100.0 °C | 205 GPa Show Material materials with Elastic modulus of 205 GPa | ||
200.0 °C | 193 GPa Show Material materials with Elastic modulus of 193 GPa | ||
300.0 °C | 185 GPa Show Material materials with Elastic modulus of 185 GPa | ||
400.0 °C | 175 GPa Show Material materials with Elastic modulus of 175 GPa | ||
Poisson's ratio | 23.0 °C | 0.29 [-] Show Material materials with Poisson's ratio of 0.29 [-] | Typical for Low Carbon Steel |
Shear modulus | 20.0 °C | 81 GPa Show Material materials with Shear modulus of 81 GPa |
Thermal
Property | Temperature | Value | Comment |
---|---|---|---|
Coefficient of thermal expansion | 100.0 °C | 1.1E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.1E-5 1/K | |
200.0 °C | 1.18E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.18E-5 1/K | ||
400.0 °C | 1.32E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.32E-5 1/K | ||
Max service temperature | 500 °C Show Material materials with Max service temperature of 500 °C | Typical for Carbon Steel | |
Max service temperature, long | -25 - 0 °C Show Material materials with Max service temperature, long of -25 - 0 °C | ||
Melting point | 1480 - 1526 °C Show Material materials with Melting point of 1480 - 1526 °C | Typical for Low Carbon Steel | |
Specific heat capacity | 20.0 °C | 460 J/(kg·K) Show Material materials with Specific heat capacity of 460 J/(kg·K) | |
100.0 °C | 480 J/(kg·K) Show Material materials with Specific heat capacity of 480 J/(kg·K) | ||
200.0 °C | 520 J/(kg·K) Show Material materials with Specific heat capacity of 520 J/(kg·K) | ||
Thermal conductivity | 20.0 °C | 58.7 W/(m·K) Show Material materials with Thermal conductivity of 58.7 W/(m·K) | |
100.0 °C | 54.4 W/(m·K) Show Material materials with Thermal conductivity of 54.4 W/(m·K) | ||
200.0 °C | 50.2 W/(m·K) Show Material materials with Thermal conductivity of 50.2 W/(m·K) | ||
400.0 °C | 44 W/(m·K) Show Material materials with Thermal conductivity of 44 W/(m·K) | ||
Electrical
Property | Temperature | Value |
---|---|---|
Electrical resistivity | 20.0 °C | 1.1E-7 Ω·m Show Material materials with Electrical resistivity of 1.1E-7 Ω·m |
Magnetic
Property | Value | Comment |
---|---|---|
Curie temperature | 770 °C Show Material materials with Curie temperature of 770 °C | Typical for Low Carbon Steel |
Chemical properties
Property | Value |
---|---|
Carbon | 0.12 - 0.18 % Show Material materials with Carbon of 0.12 - 0.18 % |
Lead | 0.15 - 0.3 % Show Material materials with Lead of 0.15 - 0.3 % |
Manganese | 0.3 - 0.6 % Show Material materials with Manganese of 0.3 - 0.6 % |
Phosphorus | 0.05 % Show Material materials with Phosphorus of 0.05 % |
Silicon | 0.4 % Show Material materials with Silicon of 0.4 % |
Sulfur | 0.045 % Show Material materials with Sulfur of 0.045 % |