General
Property | Temperature | Value |
---|---|---|
Density | 20.0 °C | 8.12 g/cm³ Show Material materials with Density of 8.12 g/cm³ |
Mechanical
Property | Temperature | Value | Comment |
---|---|---|---|
Elastic modulus | 20.0 °C | 224 GPa Show Material materials with Elastic modulus of 224 GPa | |
100.0 °C | 220 GPa Show Material materials with Elastic modulus of 220 GPa | ||
200.0 °C | 214 GPa Show Material materials with Elastic modulus of 214 GPa | ||
300.0 °C | 207 GPa Show Material materials with Elastic modulus of 207 GPa | ||
400.0 °C | 199 GPa Show Material materials with Elastic modulus of 199 GPa | ||
500.0 °C | 191 GPa Show Material materials with Elastic modulus of 191 GPa | ||
600.0 °C | 180 GPa Show Material materials with Elastic modulus of 180 GPa | ||
Poisson's ratio | 20.0 °C | 0.28 [-] Show Material materials with Poisson's ratio of 0.28 [-] | |
Shear modulus | 23.0 °C | 79 GPa Show Material materials with Shear modulus of 79 GPa | Typical for Tool And Machining Steel |
Thermal
Property | Temperature | Value | Comment |
---|---|---|---|
Coefficient of thermal expansion | -100.0 °C | 9.6E-6 1/K Show Material materials with Coefficient of thermal expansion of 9.6E-6 1/K | |
20.0 °C | 1.05E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.05E-5 1/K | ||
100.0 °C | 1.11E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.11E-5 1/K | ||
200.0 °C | 1.16E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.16E-5 1/K | ||
300.0 °C | 1.2E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.2E-5 1/K | ||
400.0 °C | 1.24E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.24E-5 1/K | ||
500.0 °C | 1.27E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.27E-5 1/K | ||
600.0 °C | 1.3E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.3E-5 1/K | ||
Melting point | 1370 - 1425 °C Show Material materials with Melting point of 1370 - 1425 °C | Typical for Tool And Machining Steel | |
Specific heat capacity | 23.0 °C | 420 - 460 J/(kg·K) Show Material materials with Specific heat capacity of 420 - 460 J/(kg·K) | Typical for Tool And Machining Steel |
Thermal conductivity | 20.0 °C | 27.6 W/(m·K) Show Material materials with Thermal conductivity of 27.6 W/(m·K) | |
100.0 °C | 27.9 W/(m·K) Show Material materials with Thermal conductivity of 27.9 W/(m·K) | ||
200.0 °C | 27.7 W/(m·K) Show Material materials with Thermal conductivity of 27.7 W/(m·K) | ||
300.0 °C | 27.5 W/(m·K) Show Material materials with Thermal conductivity of 27.5 W/(m·K) | ||
400.0 °C | 27 W/(m·K) Show Material materials with Thermal conductivity of 27 W/(m·K) | ||
500.0 °C | 26.6 W/(m·K) Show Material materials with Thermal conductivity of 26.6 W/(m·K) | ||
600.0 °C | 26.1 W/(m·K) Show Material materials with Thermal conductivity of 26.1 W/(m·K) | ||
Electrical
Property | Temperature | Value |
---|---|---|
Electrical resistivity | 20.0 °C | 5.24E-7 Ω·m Show Material materials with Electrical resistivity of 5.24E-7 Ω·m |
100.0 °C | 5.81E-7 Ω·m Show Material materials with Electrical resistivity of 5.81E-7 Ω·m | |
200.0 °C | 6.64E-7 Ω·m Show Material materials with Electrical resistivity of 6.64E-7 Ω·m | |
300.0 °C | 7.51E-7 Ω·m Show Material materials with Electrical resistivity of 7.51E-7 Ω·m | |
400.0 °C | 8.44E-7 Ω·m Show Material materials with Electrical resistivity of 8.44E-7 Ω·m | |
500.0 °C | 9.41E-7 Ω·m Show Material materials with Electrical resistivity of 9.41E-7 Ω·m | |
600.0 °C | 1.04E-6 Ω·m Show Material materials with Electrical resistivity of 1.04E-6 Ω·m | |
Chemical properties
Property | Value |
---|---|
Carbon | 0.88 - 0.96 % Show Material materials with Carbon of 0.88 - 0.96 % |
Chromium | 3.8 - 4.5 % Show Material materials with Chromium of 3.8 - 4.5 % |
Cobalt | 4.5 - 5 % Show Material materials with Cobalt of 4.5 - 5 % |
Manganese | 0.4 % Show Material materials with Manganese of 0.4 % |
Molybdenum | 4.7 - 5.2 % Show Material materials with Molybdenum of 4.7 - 5.2 % |
Phosphorus | 0.03 % Show Material materials with Phosphorus of 0.03 % |
Silicon | 0.45 % Show Material materials with Silicon of 0.45 % |
Sulfur | 0.03 % Show Material materials with Sulfur of 0.03 % |
Tungsten | 6 - 6.7 % Show Material materials with Tungsten of 6 - 6.7 % |