General
Property | Temperature | Value |
---|---|---|
Density | 20.0 °C | 7.74 g/cm³ Show Material materials with Density of 7.74 g/cm³ |
Mechanical
Property | Temperature | Value | Comment |
---|---|---|---|
Elastic modulus | 20.0 °C | 210 GPa Show Material materials with Elastic modulus of 210 GPa | |
Poisson's ratio | 20.0 °C | 0.28 [-] Show Material materials with Poisson's ratio of 0.28 [-] | |
Shear modulus | 23.0 °C | 79 GPa Show Material materials with Shear modulus of 79 GPa | Typical for Tool And Machining Steel |
Thermal
Property | Temperature | Value | Comment |
---|---|---|---|
Coefficient of thermal expansion | -100.0 °C | 1E-5 1/K Show Material materials with Coefficient of thermal expansion of 1E-5 1/K | |
20.0 °C | 1.08E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.08E-5 1/K | ||
100.0 °C | 1.13E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.13E-5 1/K | ||
200.0 °C | 1.18E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.18E-5 1/K | ||
300.0 °C | 1.23E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.23E-5 1/K | ||
400.0 °C | 1.27E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.27E-5 1/K | ||
500.0 °C | 1.3E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.3E-5 1/K | ||
600.0 °C | 1.32E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.32E-5 1/K | ||
Melting point | 1370 - 1425 °C Show Material materials with Melting point of 1370 - 1425 °C | Typical for Tool And Machining Steel | |
Specific heat capacity | 20.0 °C | 461 J/(kg·K) Show Material materials with Specific heat capacity of 461 J/(kg·K) | |
100.0 °C | 479 J/(kg·K) Show Material materials with Specific heat capacity of 479 J/(kg·K) | ||
200.0 °C | 499 J/(kg·K) Show Material materials with Specific heat capacity of 499 J/(kg·K) | ||
300.0 °C | 517 J/(kg·K) Show Material materials with Specific heat capacity of 517 J/(kg·K) | ||
400.0 °C | 536 J/(kg·K) Show Material materials with Specific heat capacity of 536 J/(kg·K) | ||
500.0 °C | 558 J/(kg·K) Show Material materials with Specific heat capacity of 558 J/(kg·K) | ||
600.0 °C | 587 J/(kg·K) Show Material materials with Specific heat capacity of 587 J/(kg·K) | ||
Thermal conductivity | 20.0 °C | 19.2 W/(m·K) Show Material materials with Thermal conductivity of 19.2 W/(m·K) | |
100.0 °C | 20.1 W/(m·K) Show Material materials with Thermal conductivity of 20.1 W/(m·K) | ||
200.0 °C | 22.4 W/(m·K) Show Material materials with Thermal conductivity of 22.4 W/(m·K) | ||
300.0 °C | 24 W/(m·K) Show Material materials with Thermal conductivity of 24 W/(m·K) | ||
400.0 °C | 25.1 W/(m·K) Show Material materials with Thermal conductivity of 25.1 W/(m·K) | ||
500.0 °C | 25.8 W/(m·K) Show Material materials with Thermal conductivity of 25.8 W/(m·K) | ||
600.0 °C | 26.1 W/(m·K) Show Material materials with Thermal conductivity of 26.1 W/(m·K) | ||
Thermal diffusivity | 20.0 °C | 5.4 mm²/s Show Material materials with Thermal diffusivity of 5.4 mm²/s | |
100.0 °C | 5.3 mm²/s Show Material materials with Thermal diffusivity of 5.3 mm²/s | ||
200.0 °C | 5.5 mm²/s Show Material materials with Thermal diffusivity of 5.5 mm²/s | ||
300.0 °C | 5.5 mm²/s Show Material materials with Thermal diffusivity of 5.5 mm²/s | ||
400.0 °C | 5.4 mm²/s Show Material materials with Thermal diffusivity of 5.4 mm²/s | ||
500.0 °C | 5 mm²/s Show Material materials with Thermal diffusivity of 5 mm²/s | ||
600.0 °C | 4.4 mm²/s Show Material materials with Thermal diffusivity of 4.4 mm²/s | ||
Electrical
Property | Temperature | Value |
---|---|---|
Electrical resistivity | 20.0 °C | 5.43E-7 Ω·m Show Material materials with Electrical resistivity of 5.43E-7 Ω·m |
100.0 °C | 6.38E-7 Ω·m Show Material materials with Electrical resistivity of 6.38E-7 Ω·m | |
200.0 °C | 7.05E-7 Ω·m Show Material materials with Electrical resistivity of 7.05E-7 Ω·m | |
300.0 °C | 7.82E-7 Ω·m Show Material materials with Electrical resistivity of 7.82E-7 Ω·m | |
400.0 °C | 8.68E-7 Ω·m Show Material materials with Electrical resistivity of 8.68E-7 Ω·m | |
500.0 °C | 9.6E-7 Ω·m Show Material materials with Electrical resistivity of 9.6E-7 Ω·m | |
600.0 °C | 1.06E-6 Ω·m Show Material materials with Electrical resistivity of 1.06E-6 Ω·m | |
Chemical properties
Property | Value |
---|---|
Carbon | 0.37 - 0.43 % Show Material materials with Carbon of 0.37 - 0.43 % |
Chromium | 4.8 - 5.5 % Show Material materials with Chromium of 4.8 - 5.5 % |
Manganese | 0.3 - 0.5 % Show Material materials with Manganese of 0.3 - 0.5 % |
Molybdenum | 1.2 - 1.5 % Show Material materials with Molybdenum of 1.2 - 1.5 % |
Phosphorus | 0.03 % Show Material materials with Phosphorus of 0.03 % |
Silicon | 0.9 - 1.2 % Show Material materials with Silicon of 0.9 - 1.2 % |
Sulfur | 0.03 % Show Material materials with Sulfur of 0.03 % |
Vanadium | 0.9 - 1.1 % Show Material materials with Vanadium of 0.9 - 1.1 % |