DIN 17440 Grade X6CrAl13 soft annealed (+A)

Want to keep this datasheet? Save it now in your required format

Description

Properties: - Al-additives reduces hardening next to the welding seam and thus the tendency for cracking - application temperature: up to 600 °C Application: - for construction of parts in petroleum industry (crack systems) - for welded parts in hydroelectric power plant construction

Related Standards

Equivalent Materials

This material data has been provided by WIAM.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValue

Density

20.0 °C

7.58 - 7.7 g/cm³

Show Material materials with Density of 7.58 - 7.7 g/cm³

Mechanical

PropertyTemperatureValueComment

Elastic modulus

20.0 °C

216 - 220 GPa

Show Material materials with Elastic modulus of 216 - 220 GPa

100.0 °C

213 - 215 GPa

Show Material materials with Elastic modulus of 213 - 215 GPa

200.0 °C

206 - 210 GPa

Show Material materials with Elastic modulus of 206 - 210 GPa

300.0 °C

198 - 205 GPa

Show Material materials with Elastic modulus of 198 - 205 GPa

400.0 °C

190 - 195 GPa

Show Material materials with Elastic modulus of 190 - 195 GPa

500.0 °C

180 GPa

Show Material materials with Elastic modulus of 180 GPa

600.0 °C

167 GPa

Show Material materials with Elastic modulus of 167 GPa

700.0 °C

150 GPa

Show Material materials with Elastic modulus of 150 GPa

Elongation

20.0 °C

20 %

Show Material materials with Elongation of 20 %

Elongation, transverse

20.0 °C

15 %

Show Material materials with Elongation, transverse of 15 %

Hardness, Brinell

20.0 °C

185 [-]

Show Material materials with Hardness, Brinell of 185 [-]

Hardness, Brinell, trans

20.0 °C

185 [-]

Show Material materials with Hardness, Brinell, trans of 185 [-]

Hardness, Vickers

20.0 °C

185 [-]

Show Material materials with Hardness, Vickers of 185 [-]

Poisson's ratio

23.0 °C

0.3 [-]

Show Material materials with Poisson's ratio of 0.3 [-]

Typical for Ferritic Stainless Steel

Shear modulus

23.0 °C

77 GPa

Show Material materials with Shear modulus of 77 GPa

Typical for Ferritic Stainless Steel

Tensile strength

20.0 °C

400 - 600 MPa

Show Material materials with Tensile strength of 400 - 600 MPa

Tensile strength, transverse

20.0 °C

400 - 600 MPa

Show Material materials with Tensile strength, transverse of 400 - 600 MPa

Yield strength

20.0 °C

250 MPa

Show Material materials with Yield strength of 250 MPa

Yield strength Rp0.2

20.0 °C

240 - 250 MPa

Show Material materials with Yield strength Rp0.2 of 240 - 250 MPa

50.0 °C

235 - 240 MPa

Show Material materials with Yield strength Rp0.2 of 235 - 240 MPa

100.0 °C

230 - 235 MPa

Show Material materials with Yield strength Rp0.2 of 230 - 235 MPa

150.0 °C

225 - 230 MPa

Show Material materials with Yield strength Rp0.2 of 225 - 230 MPa

200.0 °C

225 MPa

Show Material materials with Yield strength Rp0.2 of 225 MPa

250.0 °C

220 - 225 MPa

Show Material materials with Yield strength Rp0.2 of 220 - 225 MPa

300.0 °C

210 - 220 MPa

Show Material materials with Yield strength Rp0.2 of 210 - 220 MPa

350.0 °C

195 - 210 MPa

Show Material materials with Yield strength Rp0.2 of 195 - 210 MPa

400.0 °C

195 MPa

Show Material materials with Yield strength Rp0.2 of 195 MPa

Unlock all property charts

Yield strength Rp0.2, transverse

20.0 °C

250 MPa

Show Material materials with Yield strength Rp0.2, transverse of 250 MPa

Yield strength, transverse

20.0 °C

250 MPa

Show Material materials with Yield strength, transverse of 250 MPa

Thermal

PropertyTemperatureValueComment

Coefficient of thermal expansion

20.0 °C

1.02E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.02E-5 1/K

100.0 °C

1.05E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.05E-5 1/K

200.0 °C

1.09E-5 - 1.1E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.09E-5 - 1.1E-5 1/K

300.0 °C

1.13E-5 - 1.15E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.13E-5 - 1.15E-5 1/K

400.0 °C

1.16E-5 - 1.2E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.16E-5 - 1.2E-5 1/K

500.0 °C

1.2E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.2E-5 1/K

600.0 °C

1.22E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.22E-5 1/K

700.0 °C

1.24E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.24E-5 1/K

Unlock all property charts

Max service temperature, long

0 - 600 °C

Show Material materials with Max service temperature, long of 0 - 600 °C

Melting point

1425 - 1530 °C

Show Material materials with Melting point of 1425 - 1530 °C

Typical for Ferritic Stainless Steel

Specific heat capacity

20.0 °C

439 - 460 J/(kg·K)

Show Material materials with Specific heat capacity of 439 - 460 J/(kg·K)

100.0 °C

474 J/(kg·K)

Show Material materials with Specific heat capacity of 474 J/(kg·K)

200.0 °C

492 J/(kg·K)

Show Material materials with Specific heat capacity of 492 J/(kg·K)

300.0 °C

517 J/(kg·K)

Show Material materials with Specific heat capacity of 517 J/(kg·K)

400.0 °C

538 J/(kg·K)

Show Material materials with Specific heat capacity of 538 J/(kg·K)

500.0 °C

564 J/(kg·K)

Show Material materials with Specific heat capacity of 564 J/(kg·K)

600.0 °C

598 J/(kg·K)

Show Material materials with Specific heat capacity of 598 J/(kg·K)

700.0 °C

647 J/(kg·K)

Show Material materials with Specific heat capacity of 647 J/(kg·K)

Unlock all property charts

Thermal conductivity

20.0 °C

15.7 - 30 W/(m·K)

Show Material materials with Thermal conductivity of 15.7 - 30 W/(m·K)

100.0 °C

17.1 W/(m·K)

Show Material materials with Thermal conductivity of 17.1 W/(m·K)

200.0 °C

18.6 W/(m·K)

Show Material materials with Thermal conductivity of 18.6 W/(m·K)

300.0 °C

20 W/(m·K)

Show Material materials with Thermal conductivity of 20 W/(m·K)

400.0 °C

21.2 W/(m·K)

Show Material materials with Thermal conductivity of 21.2 W/(m·K)

500.0 °C

22.3 W/(m·K)

Show Material materials with Thermal conductivity of 22.3 W/(m·K)

600.0 °C

23.1 W/(m·K)

Show Material materials with Thermal conductivity of 23.1 W/(m·K)

700.0 °C

23.8 W/(m·K)

Show Material materials with Thermal conductivity of 23.8 W/(m·K)

Unlock all property charts

Thermal diffusivity

20.0 °C

4.7 mm²/s

Show Material materials with Thermal diffusivity of 4.7 mm²/s

100.0 °C

4.5 mm²/s

Show Material materials with Thermal diffusivity of 4.5 mm²/s

200.0 °C

4.6 mm²/s

Show Material materials with Thermal diffusivity of 4.6 mm²/s

300.0 °C

4.7 mm²/s

Show Material materials with Thermal diffusivity of 4.7 mm²/s

400.0 °C

4.5 mm²/s

Show Material materials with Thermal diffusivity of 4.5 mm²/s

500.0 °C

4.3 mm²/s

Show Material materials with Thermal diffusivity of 4.3 mm²/s

600.0 °C

3.7 mm²/s

Show Material materials with Thermal diffusivity of 3.7 mm²/s

700.0 °C

3 mm²/s

Show Material materials with Thermal diffusivity of 3 mm²/s

Unlock all property charts

Electrical

PropertyTemperatureValue

Electrical resistivity

20.0 °C

6E-7 - 9.19E-7 Ω·m

Show Material materials with Electrical resistivity of 6E-7 - 9.19E-7 Ω·m

100.0 °C

9.48E-7 Ω·m

Show Material materials with Electrical resistivity of 9.48E-7 Ω·m

200.0 °C

9.87E-7 Ω·m

Show Material materials with Electrical resistivity of 9.87E-7 Ω·m

300.0 °C

1.03E-6 Ω·m

Show Material materials with Electrical resistivity of 1.03E-6 Ω·m

400.0 °C

1.07E-6 Ω·m

Show Material materials with Electrical resistivity of 1.07E-6 Ω·m

500.0 °C

1.12E-6 Ω·m

Show Material materials with Electrical resistivity of 1.12E-6 Ω·m

600.0 °C

1.18E-6 Ω·m

Show Material materials with Electrical resistivity of 1.18E-6 Ω·m

700.0 °C

1.24E-6 Ω·m

Show Material materials with Electrical resistivity of 1.24E-6 Ω·m

Unlock all property charts

Chemical properties

PropertyValue

Aluminium

0.1 - 0.3 %

Show Material materials with Aluminium of 0.1 - 0.3 %

Carbon

0.08 %

Show Material materials with Carbon of 0.08 %

Chromium

12 - 14 %

Show Material materials with Chromium of 12 - 14 %

Manganese

1 %

Show Material materials with Manganese of 1 %

Phosphorus

0.04 - 0.05 %

Show Material materials with Phosphorus of 0.04 - 0.05 %

Silicon

1 %

Show Material materials with Silicon of 1 %

Sulfur

0.015 - 0.03 %

Show Material materials with Sulfur of 0.015 - 0.03 %