DIN 17440 Grade X6CrNiTi18-10 quenched (+Q)

Want to keep this datasheet? Save it now in your required format

Description

Properties: - is the with titanium stabilised variant of 1.4301 - thus after welding also with material thicknesses > 6 mm resistant to intergranular corrosion - due to the Ti-additive the steel is not high polishable - is certified for the construction of pressure tanks to 300 °C, if no disintegration of grains-releasing media are present, then up to 550°C is possible - the strength grades E 225, E 355 are usual. Application: - employment in large extent for welded parts in the chemical apparatus engineering - food, luxuries, fat and soap industry - in the film and photo industry, in leather and sugar factories and for houseware - in architecure for construction units with supporting function is certified (extended licence notice No. Z-30.44.1 of Institut für Bautechnik Berlin from 1 February 1994)

Related Standards

Equivalent Materials

This material data has been provided by WIAM.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValue

Density

20.0 °C

7.9 - 7.93 g/cm³

Show Material materials with Density of 7.9 - 7.93 g/cm³

Mechanical

PropertyTemperatureValue

Elastic modulus

-100.0 °C

206 GPa

Show Material materials with Elastic modulus of 206 GPa

20.0 °C

196 - 200 GPa

Show Material materials with Elastic modulus of 196 - 200 GPa

95.0 °C

193.05 GPa

Show Material materials with Elastic modulus of 193.05 GPa

100.0 °C

190 - 194 GPa

Show Material materials with Elastic modulus of 190 - 194 GPa

150.0 °C

188.23 GPa

Show Material materials with Elastic modulus of 188.23 GPa

200.0 °C

182 - 186 GPa

Show Material materials with Elastic modulus of 182 - 186 GPa

205.0 °C

182.71 GPa

Show Material materials with Elastic modulus of 182.71 GPa

260.0 °C

177.88 GPa

Show Material materials with Elastic modulus of 177.88 GPa

300.0 °C

174 - 179 GPa

Show Material materials with Elastic modulus of 174 - 179 GPa

315.0 °C

174.44 GPa

Show Material materials with Elastic modulus of 174.44 GPa

370.0 °C

168.92 GPa

Show Material materials with Elastic modulus of 168.92 GPa

400.0 °C

166 - 172 GPa

Show Material materials with Elastic modulus of 166 - 172 GPa

425.0 °C

164.1 GPa

Show Material materials with Elastic modulus of 164.1 GPa

485.0 °C

159.96 GPa

Show Material materials with Elastic modulus of 159.96 GPa

500.0 °C

158 - 165 GPa

Show Material materials with Elastic modulus of 158 - 165 GPa

540.0 °C

155.13 GPa

Show Material materials with Elastic modulus of 155.13 GPa

595.0 °C

151 GPa

Show Material materials with Elastic modulus of 151 GPa

600.0 °C

150 GPa

Show Material materials with Elastic modulus of 150 GPa

650.0 °C

146.17 GPa

Show Material materials with Elastic modulus of 146.17 GPa

700.0 °C

142 GPa

Show Material materials with Elastic modulus of 142 GPa

705.0 °C

140.65 GPa

Show Material materials with Elastic modulus of 140.65 GPa

760.0 °C

135.83 GPa

Show Material materials with Elastic modulus of 135.83 GPa

800.0 °C

134 GPa

Show Material materials with Elastic modulus of 134 GPa

815.0 °C

131.69 GPa

Show Material materials with Elastic modulus of 131.69 GPa

900.0 °C

127 GPa

Show Material materials with Elastic modulus of 127 GPa

1000.0 °C

120 GPa

Show Material materials with Elastic modulus of 120 GPa

Elongation

20.0 °C

35 - 40 %

Show Material materials with Elongation of 35 - 40 %

Elongation A80

20.0 °C

35 %

Show Material materials with Elongation A80 of 35 %

Elongation A80, transverse

20.0 °C

42 %

Show Material materials with Elongation A80, transverse of 42 %

Elongation, transverse

20.0 °C

30 - 42 %

Show Material materials with Elongation, transverse of 30 - 42 %

Poisson's ratio

20.0 °C

0.29 [-]

Show Material materials with Poisson's ratio of 0.29 [-]

95.0 °C

0.3 [-]

Show Material materials with Poisson's ratio of 0.3 [-]

150.0 °C

0.29 [-]

Show Material materials with Poisson's ratio of 0.29 [-]

205.0 °C

0.29 [-]

Show Material materials with Poisson's ratio of 0.29 [-]

260.0 °C

0.3 [-]

Show Material materials with Poisson's ratio of 0.3 [-]

315.0 °C

0.3 [-]

Show Material materials with Poisson's ratio of 0.3 [-]

370.0 °C

0.3 [-]

Show Material materials with Poisson's ratio of 0.3 [-]

425.0 °C

0.31 [-]

Show Material materials with Poisson's ratio of 0.31 [-]

485.0 °C

0.32 [-]

Show Material materials with Poisson's ratio of 0.32 [-]

540.0 °C

0.32 [-]

Show Material materials with Poisson's ratio of 0.32 [-]

595.0 °C

0.34 [-]

Show Material materials with Poisson's ratio of 0.34 [-]

650.0 °C

0.34 [-]

Show Material materials with Poisson's ratio of 0.34 [-]

705.0 °C

0.33 [-]

Show Material materials with Poisson's ratio of 0.33 [-]

760.0 °C

0.33 [-]

Show Material materials with Poisson's ratio of 0.33 [-]

815.0 °C

0.35 [-]

Show Material materials with Poisson's ratio of 0.35 [-]

Unlock all property charts

Shear modulus

20.0 °C

77.22 GPa

Show Material materials with Shear modulus of 77.22 GPa

95.0 °C

74.46 GPa

Show Material materials with Shear modulus of 74.46 GPa

150.0 °C

73.08 GPa

Show Material materials with Shear modulus of 73.08 GPa

205.0 °C

71.02 GPa

Show Material materials with Shear modulus of 71.02 GPa

260.0 °C

68.26 GPa

Show Material materials with Shear modulus of 68.26 GPa

315.0 °C

66.88 GPa

Show Material materials with Shear modulus of 66.88 GPa

370.0 °C

64.81 GPa

Show Material materials with Shear modulus of 64.81 GPa

425.0 °C

62.74 GPa

Show Material materials with Shear modulus of 62.74 GPa

485.0 °C

60.67 GPa

Show Material materials with Shear modulus of 60.67 GPa

540.0 °C

58.61 GPa

Show Material materials with Shear modulus of 58.61 GPa

595.0 °C

56.54 GPa

Show Material materials with Shear modulus of 56.54 GPa

650.0 °C

54.47 GPa

Show Material materials with Shear modulus of 54.47 GPa

705.0 °C

53.09 GPa

Show Material materials with Shear modulus of 53.09 GPa

760.0 °C

51.02 GPa

Show Material materials with Shear modulus of 51.02 GPa

815.0 °C

48.95 GPa

Show Material materials with Shear modulus of 48.95 GPa

Unlock all property charts

Tensile strength

20.0 °C

500 - 730 MPa

Show Material materials with Tensile strength of 500 - 730 MPa

Tensile strength, transverse

20.0 °C

500 - 730 MPa

Show Material materials with Tensile strength, transverse of 500 - 730 MPa

Yield strength Rp0.2

20.0 °C

200 MPa

Show Material materials with Yield strength Rp0.2 of 200 MPa

50.0 °C

190 MPa

Show Material materials with Yield strength Rp0.2 of 190 MPa

100.0 °C

176 MPa

Show Material materials with Yield strength Rp0.2 of 176 MPa

150.0 °C

167 MPa

Show Material materials with Yield strength Rp0.2 of 167 MPa

200.0 °C

157 MPa

Show Material materials with Yield strength Rp0.2 of 157 MPa

250.0 °C

147 MPa

Show Material materials with Yield strength Rp0.2 of 147 MPa

300.0 °C

136 MPa

Show Material materials with Yield strength Rp0.2 of 136 MPa

350.0 °C

130 MPa

Show Material materials with Yield strength Rp0.2 of 130 MPa

400.0 °C

125 MPa

Show Material materials with Yield strength Rp0.2 of 125 MPa

450.0 °C

121 MPa

Show Material materials with Yield strength Rp0.2 of 121 MPa

500.0 °C

119 MPa

Show Material materials with Yield strength Rp0.2 of 119 MPa

550.0 °C

118 MPa

Show Material materials with Yield strength Rp0.2 of 118 MPa

Unlock all property charts

Yield strength Rp0.2, transverse

20.0 °C

200 MPa

Show Material materials with Yield strength Rp0.2, transverse of 200 MPa

Yield strength Rp1.0

20.0 °C

235 MPa

Show Material materials with Yield strength Rp1.0 of 235 MPa

50.0 °C

222 MPa

Show Material materials with Yield strength Rp1.0 of 222 MPa

100.0 °C

208 MPa

Show Material materials with Yield strength Rp1.0 of 208 MPa

150.0 °C

195 MPa

Show Material materials with Yield strength Rp1.0 of 195 MPa

200.0 °C

185 MPa

Show Material materials with Yield strength Rp1.0 of 185 MPa

250.0 °C

175 MPa

Show Material materials with Yield strength Rp1.0 of 175 MPa

300.0 °C

165 - 167 MPa

Show Material materials with Yield strength Rp1.0 of 165 - 167 MPa

350.0 °C

161 MPa

Show Material materials with Yield strength Rp1.0 of 161 MPa

400.0 °C

156 MPa

Show Material materials with Yield strength Rp1.0 of 156 MPa

450.0 °C

152 MPa

Show Material materials with Yield strength Rp1.0 of 152 MPa

500.0 °C

149 MPa

Show Material materials with Yield strength Rp1.0 of 149 MPa

550.0 °C

147 MPa

Show Material materials with Yield strength Rp1.0 of 147 MPa

Unlock all property charts

Yield strength Rp1.0, transverse

20.0 °C

235 MPa

Show Material materials with Yield strength Rp1.0, transverse of 235 MPa

Thermal

PropertyTemperatureValueComment

Coefficient of thermal expansion

-100.0 °C

1.49E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.49E-5 1/K

20.0 °C

1.61E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.61E-5 1/K

100.0 °C

1.6E-5 - 1.67E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.6E-5 - 1.67E-5 1/K

200.0 °C

1.7E-5 - 1.72E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.7E-5 - 1.72E-5 1/K

300.0 °C

1.7E-5 - 1.77E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.7E-5 - 1.77E-5 1/K

400.0 °C

1.8E-5 - 1.81E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.8E-5 - 1.81E-5 1/K

500.0 °C

1.8E-5 - 1.84E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.8E-5 - 1.84E-5 1/K

600.0 °C

1.88E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.88E-5 1/K

700.0 °C

1.91E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.91E-5 1/K

800.0 °C

1.94E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.94E-5 1/K

900.0 °C

1.97E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.97E-5 1/K

1000.0 °C

2E-5 1/K

Show Material materials with Coefficient of thermal expansion of 2E-5 1/K

Unlock all property charts

Max service temperature, long

0 - 550 °C

Show Material materials with Max service temperature, long of 0 - 550 °C

Melting point

1230 - 1480 °C

Show Material materials with Melting point of 1230 - 1480 °C

Typical for Austenitic Stainless Steel

Specific heat capacity

-100.0 °C

440 J/(kg·K)

Show Material materials with Specific heat capacity of 440 J/(kg·K)

20.0 °C

472 - 500 J/(kg·K)

Show Material materials with Specific heat capacity of 472 - 500 J/(kg·K)

100.0 °C

487 J/(kg·K)

Show Material materials with Specific heat capacity of 487 J/(kg·K)

200.0 °C

503 J/(kg·K)

Show Material materials with Specific heat capacity of 503 J/(kg·K)

300.0 °C

512 J/(kg·K)

Show Material materials with Specific heat capacity of 512 J/(kg·K)

400.0 °C

520 J/(kg·K)

Show Material materials with Specific heat capacity of 520 J/(kg·K)

500.0 °C

530 J/(kg·K)

Show Material materials with Specific heat capacity of 530 J/(kg·K)

600.0 °C

541 J/(kg·K)

Show Material materials with Specific heat capacity of 541 J/(kg·K)

700.0 °C

551 J/(kg·K)

Show Material materials with Specific heat capacity of 551 J/(kg·K)

800.0 °C

559 J/(kg·K)

Show Material materials with Specific heat capacity of 559 J/(kg·K)

900.0 °C

565 J/(kg·K)

Show Material materials with Specific heat capacity of 565 J/(kg·K)

1000.0 °C

571 J/(kg·K)

Show Material materials with Specific heat capacity of 571 J/(kg·K)

Unlock all property charts

Thermal conductivity

20.0 °C

14.3 - 15 W/(m·K)

Show Material materials with Thermal conductivity of 14.3 - 15 W/(m·K)

100.0 °C

15.8 W/(m·K)

Show Material materials with Thermal conductivity of 15.8 W/(m·K)

200.0 °C

17.5 W/(m·K)

Show Material materials with Thermal conductivity of 17.5 W/(m·K)

300.0 °C

19 W/(m·K)

Show Material materials with Thermal conductivity of 19 W/(m·K)

400.0 °C

20.5 W/(m·K)

Show Material materials with Thermal conductivity of 20.5 W/(m·K)

500.0 °C

21.9 W/(m·K)

Show Material materials with Thermal conductivity of 21.9 W/(m·K)

600.0 °C

23.3 W/(m·K)

Show Material materials with Thermal conductivity of 23.3 W/(m·K)

700.0 °C

24.6 W/(m·K)

Show Material materials with Thermal conductivity of 24.6 W/(m·K)

800.0 °C

26 W/(m·K)

Show Material materials with Thermal conductivity of 26 W/(m·K)

900.0 °C

27.4 W/(m·K)

Show Material materials with Thermal conductivity of 27.4 W/(m·K)

1000.0 °C

28.8 W/(m·K)

Show Material materials with Thermal conductivity of 28.8 W/(m·K)

Unlock all property charts

Thermal diffusivity

20.0 °C

3.8 mm²/s

Show Material materials with Thermal diffusivity of 3.8 mm²/s

100.0 °C

4 mm²/s

Show Material materials with Thermal diffusivity of 4 mm²/s

200.0 °C

4.2 mm²/s

Show Material materials with Thermal diffusivity of 4.2 mm²/s

300.0 °C

4.6 mm²/s

Show Material materials with Thermal diffusivity of 4.6 mm²/s

400.0 °C

4.8 mm²/s

Show Material materials with Thermal diffusivity of 4.8 mm²/s

500.0 °C

4.9 mm²/s

Show Material materials with Thermal diffusivity of 4.9 mm²/s

600.0 °C

5 mm²/s

Show Material materials with Thermal diffusivity of 5 mm²/s

700.0 °C

5.3 mm²/s

Show Material materials with Thermal diffusivity of 5.3 mm²/s

800.0 °C

5.6 mm²/s

Show Material materials with Thermal diffusivity of 5.6 mm²/s

900.0 °C

5.9 mm²/s

Show Material materials with Thermal diffusivity of 5.9 mm²/s

1000.0 °C

6 mm²/s

Show Material materials with Thermal diffusivity of 6 mm²/s

Unlock all property charts

Electrical

PropertyTemperatureValue

Electrical resistivity

20.0 °C

7.1E-7 - 7.3E-7 Ω·m

Show Material materials with Electrical resistivity of 7.1E-7 - 7.3E-7 Ω·m

100.0 °C

7.76E-7 Ω·m

Show Material materials with Electrical resistivity of 7.76E-7 Ω·m

200.0 °C

8.49E-7 Ω·m

Show Material materials with Electrical resistivity of 8.49E-7 Ω·m

300.0 °C

9.14E-7 Ω·m

Show Material materials with Electrical resistivity of 9.14E-7 Ω·m

400.0 °C

9.71E-7 Ω·m

Show Material materials with Electrical resistivity of 9.71E-7 Ω·m

500.0 °C

1.02E-6 Ω·m

Show Material materials with Electrical resistivity of 1.02E-6 Ω·m

600.0 °C

1.07E-6 Ω·m

Show Material materials with Electrical resistivity of 1.07E-6 Ω·m

700.0 °C

1.1E-6 Ω·m

Show Material materials with Electrical resistivity of 1.1E-6 Ω·m

800.0 °C

1.14E-6 Ω·m

Show Material materials with Electrical resistivity of 1.14E-6 Ω·m

900.0 °C

1.17E-6 Ω·m

Show Material materials with Electrical resistivity of 1.17E-6 Ω·m

1000.0 °C

1.19E-6 Ω·m

Show Material materials with Electrical resistivity of 1.19E-6 Ω·m

Unlock all property charts

Chemical properties

PropertyValue

Carbon

0.08 %

Show Material materials with Carbon of 0.08 %

Chromium

17 - 19 %

Show Material materials with Chromium of 17 - 19 %

Manganese

2 %

Show Material materials with Manganese of 2 %

Nickel

9 - 12 %

Show Material materials with Nickel of 9 - 12 %

Phosphorus

0.05 %

Show Material materials with Phosphorus of 0.05 %

Silicon

1 %

Show Material materials with Silicon of 1 %

Sulfur

0.015 - 0.03 %

Show Material materials with Sulfur of 0.015 - 0.03 %

Titanium

0.7 %

Show Material materials with Titanium of 0.7 %