General
Property | Temperature | Value |
---|---|---|
Density | 20.0 °C | 7.98 - 8.01 g/cm³ Show Material materials with Density of 7.98 - 8.01 g/cm³ |
Mechanical
Property | Temperature | Value |
---|---|---|
Elastic modulus | -100.0 °C | 206 GPa Show Material materials with Elastic modulus of 206 GPa |
20.0 °C | 196 - 200 GPa Show Material materials with Elastic modulus of 196 - 200 GPa | |
100.0 °C | 190 - 194 GPa Show Material materials with Elastic modulus of 190 - 194 GPa | |
200.0 °C | 182 - 186 GPa Show Material materials with Elastic modulus of 182 - 186 GPa | |
300.0 °C | 174 - 179 GPa Show Material materials with Elastic modulus of 174 - 179 GPa | |
400.0 °C | 166 - 172 GPa Show Material materials with Elastic modulus of 166 - 172 GPa | |
500.0 °C | 158 - 165 GPa Show Material materials with Elastic modulus of 158 - 165 GPa | |
600.0 °C | 150 GPa Show Material materials with Elastic modulus of 150 GPa | |
700.0 °C | 142 GPa Show Material materials with Elastic modulus of 142 GPa | |
800.0 °C | 134 GPa Show Material materials with Elastic modulus of 134 GPa | |
Elongation | 20.0 °C | 35 % Show Material materials with Elongation of 35 % |
Elongation, transverse | 20.0 °C | 30 % Show Material materials with Elongation, transverse of 30 % |
Poisson's ratio | 20.0 °C | 0.28 [-] Show Material materials with Poisson's ratio of 0.28 [-] |
Shear modulus | 20.0 °C | 77.3 GPa Show Material materials with Shear modulus of 77.3 GPa |
Tensile strength | 20.0 °C | 580 - 800 MPa Show Material materials with Tensile strength of 580 - 800 MPa |
Tensile strength, transverse | 20.0 °C | 580 - 800 MPa Show Material materials with Tensile strength, transverse of 580 - 800 MPa |
Yield strength | 20.0 °C | 295 MPa Show Material materials with Yield strength of 295 MPa |
Yield strength Rp0.2 | 20.0 °C | 295 MPa Show Material materials with Yield strength Rp0.2 of 295 MPa |
50.0 °C | 265 MPa Show Material materials with Yield strength Rp0.2 of 265 MPa | |
100.0 °C | 225 MPa Show Material materials with Yield strength Rp0.2 of 225 MPa | |
150.0 °C | 197 MPa Show Material materials with Yield strength Rp0.2 of 197 MPa | |
200.0 °C | 178 MPa Show Material materials with Yield strength Rp0.2 of 178 MPa | |
250.0 °C | 165 MPa Show Material materials with Yield strength Rp0.2 of 165 MPa | |
300.0 °C | 155 MPa Show Material materials with Yield strength Rp0.2 of 155 MPa | |
350.0 °C | 150 MPa Show Material materials with Yield strength Rp0.2 of 150 MPa | |
400.0 °C | 145 MPa Show Material materials with Yield strength Rp0.2 of 145 MPa | |
450.0 °C | 140 MPa Show Material materials with Yield strength Rp0.2 of 140 MPa | |
500.0 °C | 138 MPa Show Material materials with Yield strength Rp0.2 of 138 MPa | |
550.0 °C | 136 MPa Show Material materials with Yield strength Rp0.2 of 136 MPa | |
Yield strength Rp0.2, transverse | 20.0 °C | 295 MPa Show Material materials with Yield strength Rp0.2, transverse of 295 MPa |
Yield strength Rp1.0 | 20.0 °C | 330 MPa Show Material materials with Yield strength Rp1.0 of 330 MPa |
50.0 °C | 300 MPa Show Material materials with Yield strength Rp1.0 of 300 MPa | |
100.0 °C | 260 MPa Show Material materials with Yield strength Rp1.0 of 260 MPa | |
150.0 °C | 227 MPa Show Material materials with Yield strength Rp1.0 of 227 MPa | |
200.0 °C | 208 MPa Show Material materials with Yield strength Rp1.0 of 208 MPa | |
250.0 °C | 195 MPa Show Material materials with Yield strength Rp1.0 of 195 MPa | |
300.0 °C | 185 MPa Show Material materials with Yield strength Rp1.0 of 185 MPa | |
350.0 °C | 180 MPa Show Material materials with Yield strength Rp1.0 of 180 MPa | |
400.0 °C | 175 MPa Show Material materials with Yield strength Rp1.0 of 175 MPa | |
450.0 °C | 170 MPa Show Material materials with Yield strength Rp1.0 of 170 MPa | |
500.0 °C | 168 MPa Show Material materials with Yield strength Rp1.0 of 168 MPa | |
550.0 °C | 166 MPa Show Material materials with Yield strength Rp1.0 of 166 MPa | |
Yield strength Rp1.0, transverse | 20.0 °C | 330 MPa Show Material materials with Yield strength Rp1.0, transverse of 330 MPa |
Yield strength, transverse | 20.0 °C | 295 MPa Show Material materials with Yield strength, transverse of 295 MPa |
Thermal
Property | Temperature | Value | Comment |
---|---|---|---|
Coefficient of thermal expansion | -100.0 °C | 1.49E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.49E-5 1/K | |
20.0 °C | 1.61E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.61E-5 1/K | ||
100.0 °C | 1.65E-5 - 1.67E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.65E-5 - 1.67E-5 1/K | ||
200.0 °C | 1.72E-5 - 1.75E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.72E-5 - 1.75E-5 1/K | ||
300.0 °C | 1.75E-5 - 1.77E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.75E-5 - 1.77E-5 1/K | ||
400.0 °C | 1.81E-5 - 1.85E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.81E-5 - 1.85E-5 1/K | ||
500.0 °C | 1.84E-5 - 1.85E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.84E-5 - 1.85E-5 1/K | ||
600.0 °C | 1.88E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.88E-5 1/K | ||
700.0 °C | 1.91E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.91E-5 1/K | ||
800.0 °C | 1.94E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.94E-5 1/K | ||
900.0 °C | 1.97E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.97E-5 1/K | ||
1000.0 °C | 2E-5 1/K Show Material materials with Coefficient of thermal expansion of 2E-5 1/K | ||
Max service temperature, long | -270 - 0 °C Show Material materials with Max service temperature, long of -270 - 0 °C | ||
Melting point | 1230 - 1480 °C Show Material materials with Melting point of 1230 - 1480 °C | Typical for Austenitic Stainless Steel | |
Specific heat capacity | -100.0 °C | 440 J/(kg·K) Show Material materials with Specific heat capacity of 440 J/(kg·K) | |
20.0 °C | 472 - 500 J/(kg·K) Show Material materials with Specific heat capacity of 472 - 500 J/(kg·K) | ||
100.0 °C | 487 J/(kg·K) Show Material materials with Specific heat capacity of 487 J/(kg·K) | ||
200.0 °C | 503 J/(kg·K) Show Material materials with Specific heat capacity of 503 J/(kg·K) | ||
300.0 °C | 512 J/(kg·K) Show Material materials with Specific heat capacity of 512 J/(kg·K) | ||
400.0 °C | 520 J/(kg·K) Show Material materials with Specific heat capacity of 520 J/(kg·K) | ||
500.0 °C | 530 J/(kg·K) Show Material materials with Specific heat capacity of 530 J/(kg·K) | ||
600.0 °C | 541 J/(kg·K) Show Material materials with Specific heat capacity of 541 J/(kg·K) | ||
700.0 °C | 551 J/(kg·K) Show Material materials with Specific heat capacity of 551 J/(kg·K) | ||
800.0 °C | 559 J/(kg·K) Show Material materials with Specific heat capacity of 559 J/(kg·K) | ||
900.0 °C | 565 J/(kg·K) Show Material materials with Specific heat capacity of 565 J/(kg·K) | ||
1000.0 °C | 571 J/(kg·K) Show Material materials with Specific heat capacity of 571 J/(kg·K) | ||
Thermal conductivity | 20.0 °C | 13.5 - 15 W/(m·K) Show Material materials with Thermal conductivity of 13.5 - 15 W/(m·K) | |
100.0 °C | 14.9 W/(m·K) Show Material materials with Thermal conductivity of 14.9 W/(m·K) | ||
200.0 °C | 16.7 W/(m·K) Show Material materials with Thermal conductivity of 16.7 W/(m·K) | ||
300.0 °C | 18.3 W/(m·K) Show Material materials with Thermal conductivity of 18.3 W/(m·K) | ||
400.0 °C | 19.8 W/(m·K) Show Material materials with Thermal conductivity of 19.8 W/(m·K) | ||
500.0 °C | 21.3 W/(m·K) Show Material materials with Thermal conductivity of 21.3 W/(m·K) | ||
600.0 °C | 22.7 W/(m·K) Show Material materials with Thermal conductivity of 22.7 W/(m·K) | ||
700.0 °C | 24.2 W/(m·K) Show Material materials with Thermal conductivity of 24.2 W/(m·K) | ||
800.0 °C | 25.6 W/(m·K) Show Material materials with Thermal conductivity of 25.6 W/(m·K) | ||
Thermal diffusivity | 20.0 °C | 3.6 mm²/s Show Material materials with Thermal diffusivity of 3.6 mm²/s | |
100.0 °C | 3.7 mm²/s Show Material materials with Thermal diffusivity of 3.7 mm²/s | ||
200.0 °C | 4 mm²/s Show Material materials with Thermal diffusivity of 4 mm²/s | ||
300.0 °C | 4.4 mm²/s Show Material materials with Thermal diffusivity of 4.4 mm²/s | ||
400.0 °C | 4.6 mm²/s Show Material materials with Thermal diffusivity of 4.6 mm²/s | ||
500.0 °C | 4.7 mm²/s Show Material materials with Thermal diffusivity of 4.7 mm²/s | ||
600.0 °C | 4.9 mm²/s Show Material materials with Thermal diffusivity of 4.9 mm²/s | ||
700.0 °C | 5.2 mm²/s Show Material materials with Thermal diffusivity of 5.2 mm²/s | ||
800.0 °C | 5.5 mm²/s Show Material materials with Thermal diffusivity of 5.5 mm²/s | ||
Electrical
Property | Temperature | Value |
---|---|---|
Electrical resistivity | 20.0 °C | 7.5E-7 - 7.75E-7 Ω·m Show Material materials with Electrical resistivity of 7.5E-7 - 7.75E-7 Ω·m |
100.0 °C | 8.42E-7 Ω·m Show Material materials with Electrical resistivity of 8.42E-7 Ω·m | |
200.0 °C | 9.04E-7 Ω·m Show Material materials with Electrical resistivity of 9.04E-7 Ω·m | |
300.0 °C | 9.62E-7 Ω·m Show Material materials with Electrical resistivity of 9.62E-7 Ω·m | |
400.0 °C | 1.01E-6 Ω·m Show Material materials with Electrical resistivity of 1.01E-6 Ω·m | |
500.0 °C | 1.06E-6 Ω·m Show Material materials with Electrical resistivity of 1.06E-6 Ω·m | |
600.0 °C | 1.1E-6 Ω·m Show Material materials with Electrical resistivity of 1.1E-6 Ω·m | |
700.0 °C | 1.13E-6 Ω·m Show Material materials with Electrical resistivity of 1.13E-6 Ω·m | |
800.0 °C | 1.16E-6 Ω·m Show Material materials with Electrical resistivity of 1.16E-6 Ω·m | |
Chemical properties
Property | Value |
---|---|
Carbon | 0.03 - 0.07 % Show Material materials with Carbon of 0.03 - 0.07 % |
Chromium | 16.5 - 18.5 % Show Material materials with Chromium of 16.5 - 18.5 % |
Manganese | 2 % Show Material materials with Manganese of 2 % |
Molybdenum | 2.5 - 3 % Show Material materials with Molybdenum of 2.5 - 3 % |
Nickel | 11 - 14.5 % Show Material materials with Nickel of 11 - 14.5 % |
Nitrogen | 0.12 - 0.22 % Show Material materials with Nitrogen of 0.12 - 0.22 % |
Phosphorus | 0.05 - 0.45 % Show Material materials with Phosphorus of 0.05 - 0.45 % |
Silicon | 1 % Show Material materials with Silicon of 1 % |
Sulfur | 0.015 - 0.025 % Show Material materials with Sulfur of 0.015 - 0.025 % |