DIN 17440 Grade X3CrTi17 soft annealed (+A)

Want to keep this datasheet? Save it now in your required format

Description

The for pressure vessels approved material X3CrTi17, mat. no. 1.4510, has an similar corrosion behaviour like the X6Cr17 (1.4016). The steel is resistant to intercrystalline corrosion in the delivery condition and also in the welded condition. It is higher resistant to stress corrosion in hot lyes and weak chloride containing waters. Because of the Ti-content there is no danger for intercrystalline corrosion after welding. Thats why the steel is not high polishable. According DIN 17440 : 1996-09 it is used for flat products and rods and drawn wire and acc. DIN 17441 : 1997-02 for cold rolled strips and slit strips for pressure vessels. For the application acc. DIN 17440 : 1985-07 (X 6 CrTi 17) resp. acc. DIN EN 10088-1,-2,-3 : 1995-08 (X3CrTi17) applies: application for welded parts in washing machines (lye bins) and partially in the chemical apparatus engineering (weak acids), in the milk industry, food industry, brewery industry, textile industry and cosmetic industry.

Related Standards

Equivalent Materials

This material data has been provided by WIAM.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValue

Density

20.0 °C

7.56 - 7.7 g/cm³

Show Material materials with Density of 7.56 - 7.7 g/cm³

Mechanical

PropertyTemperatureValueComment

Elastic modulus

20.0 °C

218 - 220 GPa

Show Material materials with Elastic modulus of 218 - 220 GPa

100.0 °C

213 - 218 GPa

Show Material materials with Elastic modulus of 213 - 218 GPa

200.0 °C

206 - 212 GPa

Show Material materials with Elastic modulus of 206 - 212 GPa

300.0 °C

198 - 205 GPa

Show Material materials with Elastic modulus of 198 - 205 GPa

400.0 °C

190 - 197 GPa

Show Material materials with Elastic modulus of 190 - 197 GPa

500.0 °C

180 GPa

Show Material materials with Elastic modulus of 180 GPa

600.0 °C

167 GPa

Show Material materials with Elastic modulus of 167 GPa

700.0 °C

150 GPa

Show Material materials with Elastic modulus of 150 GPa

Elongation

20.0 °C

20 - 23 %

Show Material materials with Elongation of 20 - 23 %

Elongation A80

20.0 °C

18 - 23 %

Show Material materials with Elongation A80 of 18 - 23 %

Elongation, transverse

20.0 °C

18 %

Show Material materials with Elongation, transverse of 18 %

Hardness, Brinell

20.0 °C

185 [-]

Show Material materials with Hardness, Brinell of 185 [-]

Hardness, Brinell, trans

20.0 °C

185 [-]

Show Material materials with Hardness, Brinell, trans of 185 [-]

Hardness, Vickers

20.0 °C

185 [-]

Show Material materials with Hardness, Vickers of 185 [-]

Poisson's ratio

23.0 °C

0.3 [-]

Show Material materials with Poisson's ratio of 0.3 [-]

Typical for Ferritic Stainless Steel

Shear modulus

23.0 °C

77 GPa

Show Material materials with Shear modulus of 77 GPa

Typical for Ferritic Stainless Steel

Tensile strength

20.0 °C

420 - 600 MPa

Show Material materials with Tensile strength of 420 - 600 MPa

Tensile strength, transverse

20.0 °C

430 - 600 MPa

Show Material materials with Tensile strength, transverse of 430 - 600 MPa

Yield strength

20.0 °C

270 MPa

Show Material materials with Yield strength of 270 MPa

Yield strength Rp0.2

20.0 °C

230 - 270 MPa

Show Material materials with Yield strength Rp0.2 of 230 - 270 MPa

100.0 °C

195 MPa

Show Material materials with Yield strength Rp0.2 of 195 MPa

150.0 °C

190 MPa

Show Material materials with Yield strength Rp0.2 of 190 MPa

200.0 °C

185 MPa

Show Material materials with Yield strength Rp0.2 of 185 MPa

250.0 °C

175 MPa

Show Material materials with Yield strength Rp0.2 of 175 MPa

300.0 °C

165 MPa

Show Material materials with Yield strength Rp0.2 of 165 MPa

350.0 °C

155 MPa

Show Material materials with Yield strength Rp0.2 of 155 MPa

Unlock all property charts

Yield strength Rp0.2, transverse

20.0 °C

270 MPa

Show Material materials with Yield strength Rp0.2, transverse of 270 MPa

Yield strength, transverse

20.0 °C

270 MPa

Show Material materials with Yield strength, transverse of 270 MPa

Thermal

PropertyTemperatureValueComment

Coefficient of thermal expansion

20.0 °C

9.9E-6 1/K

Show Material materials with Coefficient of thermal expansion of 9.9E-6 1/K

100.0 °C

1E-5 - 1.03E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1E-5 - 1.03E-5 1/K

200.0 °C

1E-5 - 1.08E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1E-5 - 1.08E-5 1/K

300.0 °C

1.05E-5 - 1.12E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.05E-5 - 1.12E-5 1/K

400.0 °C

1.05E-5 - 1.16E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.05E-5 - 1.16E-5 1/K

500.0 °C

1.1E-5 - 1.19E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.1E-5 - 1.19E-5 1/K

600.0 °C

1.21E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.21E-5 1/K

700.0 °C

1.24E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.24E-5 1/K

800.0 °C

1.29E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.29E-5 1/K

Unlock all property charts

Melting point

1425 - 1530 °C

Show Material materials with Melting point of 1425 - 1530 °C

Typical for Ferritic Stainless Steel

Specific heat capacity

20.0 °C

450 - 460 J/(kg·K)

Show Material materials with Specific heat capacity of 450 - 460 J/(kg·K)

100.0 °C

482 J/(kg·K)

Show Material materials with Specific heat capacity of 482 J/(kg·K)

200.0 °C

506 J/(kg·K)

Show Material materials with Specific heat capacity of 506 J/(kg·K)

300.0 °C

525 J/(kg·K)

Show Material materials with Specific heat capacity of 525 J/(kg·K)

400.0 °C

547 J/(kg·K)

Show Material materials with Specific heat capacity of 547 J/(kg·K)

500.0 °C

576 J/(kg·K)

Show Material materials with Specific heat capacity of 576 J/(kg·K)

600.0 °C

616 J/(kg·K)

Show Material materials with Specific heat capacity of 616 J/(kg·K)

Unlock all property charts

Thermal conductivity

20.0 °C

16 - 25 W/(m·K)

Show Material materials with Thermal conductivity of 16 - 25 W/(m·K)

100.0 °C

17.2 W/(m·K)

Show Material materials with Thermal conductivity of 17.2 W/(m·K)

200.0 °C

18.6 W/(m·K)

Show Material materials with Thermal conductivity of 18.6 W/(m·K)

300.0 °C

20 W/(m·K)

Show Material materials with Thermal conductivity of 20 W/(m·K)

400.0 °C

21.2 W/(m·K)

Show Material materials with Thermal conductivity of 21.2 W/(m·K)

500.0 °C

22.3 W/(m·K)

Show Material materials with Thermal conductivity of 22.3 W/(m·K)

600.0 °C

23.3 W/(m·K)

Show Material materials with Thermal conductivity of 23.3 W/(m·K)

700.0 °C

24.1 W/(m·K)

Show Material materials with Thermal conductivity of 24.1 W/(m·K)

800.0 °C

25.5 W/(m·K)

Show Material materials with Thermal conductivity of 25.5 W/(m·K)

900.0 °C

26.9 W/(m·K)

Show Material materials with Thermal conductivity of 26.9 W/(m·K)

1000.0 °C

28.3 W/(m·K)

Show Material materials with Thermal conductivity of 28.3 W/(m·K)

Unlock all property charts

Thermal diffusivity

20.0 °C

4.7 mm²/s

Show Material materials with Thermal diffusivity of 4.7 mm²/s

100.0 °C

4.5 mm²/s

Show Material materials with Thermal diffusivity of 4.5 mm²/s

200.0 °C

4.5 mm²/s

Show Material materials with Thermal diffusivity of 4.5 mm²/s

300.0 °C

4.6 mm²/s

Show Material materials with Thermal diffusivity of 4.6 mm²/s

400.0 °C

4.4 mm²/s

Show Material materials with Thermal diffusivity of 4.4 mm²/s

500.0 °C

4.1 mm²/s

Show Material materials with Thermal diffusivity of 4.1 mm²/s

600.0 °C

3.6 mm²/s

Show Material materials with Thermal diffusivity of 3.6 mm²/s

Unlock all property charts

Electrical

PropertyTemperatureValue

Electrical resistivity

20.0 °C

6E-7 - 9.06E-7 Ω·m

Show Material materials with Electrical resistivity of 6E-7 - 9.06E-7 Ω·m

100.0 °C

9.42E-7 Ω·m

Show Material materials with Electrical resistivity of 9.42E-7 Ω·m

200.0 °C

9.87E-7 Ω·m

Show Material materials with Electrical resistivity of 9.87E-7 Ω·m

300.0 °C

1.03E-6 Ω·m

Show Material materials with Electrical resistivity of 1.03E-6 Ω·m

400.0 °C

1.08E-6 Ω·m

Show Material materials with Electrical resistivity of 1.08E-6 Ω·m

500.0 °C

1.12E-6 Ω·m

Show Material materials with Electrical resistivity of 1.12E-6 Ω·m

600.0 °C

1.18E-6 Ω·m

Show Material materials with Electrical resistivity of 1.18E-6 Ω·m

700.0 °C

1.22E-6 Ω·m

Show Material materials with Electrical resistivity of 1.22E-6 Ω·m

800.0 °C

1.24E-6 Ω·m

Show Material materials with Electrical resistivity of 1.24E-6 Ω·m

900.0 °C

1.26E-6 Ω·m

Show Material materials with Electrical resistivity of 1.26E-6 Ω·m

1000.0 °C

1.27E-6 Ω·m

Show Material materials with Electrical resistivity of 1.27E-6 Ω·m

Unlock all property charts

Chemical properties

PropertyValue

Carbon

0.05 %

Show Material materials with Carbon of 0.05 %

Chromium

16 - 18 %

Show Material materials with Chromium of 16 - 18 %

Manganese

1 %

Show Material materials with Manganese of 1 %

Phosphorus

0.04 %

Show Material materials with Phosphorus of 0.04 %

Silicon

1 %

Show Material materials with Silicon of 1 %

Sulfur

0.015 - 0.03 %

Show Material materials with Sulfur of 0.015 - 0.03 %