EN 10216-5 Grade X5NiCrAlTi31-20 recrystallization annealed (+RA)

Want to keep this datasheet? Save it now in your required format

Description

Highly creep resistant, heat resistant steel as a variant of the heat resistant steel X 10 NiCrAlTi 32 20. Operation temperature: 500 to 700 degrees C.

Related Standards

Equivalent Materials

This material data has been provided by WIAM.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValue

Density

20.0 °C

7.94 g/cm³

Show Material materials with Density of 7.94 g/cm³

Mechanical

PropertyTemperatureValueComment

Elastic modulus

-100.0 °C

201 GPa

Show Material materials with Elastic modulus of 201 GPa

20.0 °C

194 GPa

Show Material materials with Elastic modulus of 194 GPa

100.0 °C

189 GPa

Show Material materials with Elastic modulus of 189 GPa

200.0 °C

183 GPa

Show Material materials with Elastic modulus of 183 GPa

300.0 °C

177 GPa

Show Material materials with Elastic modulus of 177 GPa

400.0 °C

170 GPa

Show Material materials with Elastic modulus of 170 GPa

500.0 °C

163 GPa

Show Material materials with Elastic modulus of 163 GPa

600.0 °C

156 GPa

Show Material materials with Elastic modulus of 156 GPa

700.0 °C

149 GPa

Show Material materials with Elastic modulus of 149 GPa

800.0 °C

141 GPa

Show Material materials with Elastic modulus of 141 GPa

900.0 °C

134 GPa

Show Material materials with Elastic modulus of 134 GPa

1000.0 °C

127 GPa

Show Material materials with Elastic modulus of 127 GPa

Elongation

20.0 °C

35 %

Show Material materials with Elongation of 35 %

Elongation, transverse

20.0 °C

30 %

Show Material materials with Elongation, transverse of 30 %

Poisson's ratio

23.0 °C

0.3 [-]

Show Material materials with Poisson's ratio of 0.3 [-]

Typical for Austenitic Stainless Steel

Shear modulus

23.0 °C

77 GPa

Show Material materials with Shear modulus of 77 GPa

Typical for Austenitic Stainless Steel

Tensile strength

20.0 °C

500 - 750 MPa

Show Material materials with Tensile strength of 500 - 750 MPa

Tensile strength, transverse

20.0 °C

500 - 750 MPa

Show Material materials with Tensile strength, transverse of 500 - 750 MPa

Yield strength Rp0.2

20.0 °C

210 MPa

Show Material materials with Yield strength Rp0.2 of 210 MPa

100.0 °C

180 MPa

Show Material materials with Yield strength Rp0.2 of 180 MPa

200.0 °C

160 MPa

Show Material materials with Yield strength Rp0.2 of 160 MPa

300.0 °C

145 MPa

Show Material materials with Yield strength Rp0.2 of 145 MPa

400.0 °C

130 MPa

Show Material materials with Yield strength Rp0.2 of 130 MPa

500.0 °C

120 MPa

Show Material materials with Yield strength Rp0.2 of 120 MPa

550.0 °C

115 MPa

Show Material materials with Yield strength Rp0.2 of 115 MPa

600.0 °C

110 MPa

Show Material materials with Yield strength Rp0.2 of 110 MPa

Unlock all property charts

Yield strength Rp0.2, transverse

20.0 °C

210 MPa

Show Material materials with Yield strength Rp0.2, transverse of 210 MPa

Yield strength Rp1.0

20.0 °C

240 MPa

Show Material materials with Yield strength Rp1.0 of 240 MPa

100.0 °C

205 MPa

Show Material materials with Yield strength Rp1.0 of 205 MPa

200.0 °C

180 MPa

Show Material materials with Yield strength Rp1.0 of 180 MPa

300.0 °C

165 MPa

Show Material materials with Yield strength Rp1.0 of 165 MPa

400.0 °C

155 MPa

Show Material materials with Yield strength Rp1.0 of 155 MPa

500.0 °C

145 MPa

Show Material materials with Yield strength Rp1.0 of 145 MPa

550.0 °C

140 MPa

Show Material materials with Yield strength Rp1.0 of 140 MPa

600.0 °C

135 MPa

Show Material materials with Yield strength Rp1.0 of 135 MPa

Unlock all property charts

Yield strength Rp1.0, transverse

20.0 °C

240 MPa

Show Material materials with Yield strength Rp1.0, transverse of 240 MPa

Thermal

PropertyTemperatureValueComment

Coefficient of thermal expansion

-100.0 °C

1.36E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.36E-5 1/K

20.0 °C

1.46E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.46E-5 1/K

100.0 °C

1.51E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.51E-5 1/K

200.0 °C

1.57E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.57E-5 1/K

300.0 °C

1.62E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.62E-5 1/K

400.0 °C

1.66E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.66E-5 1/K

500.0 °C

1.7E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.7E-5 1/K

600.0 °C

1.74E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.74E-5 1/K

700.0 °C

1.77E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.77E-5 1/K

800.0 °C

1.8E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.8E-5 1/K

900.0 °C

1.83E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.83E-5 1/K

1000.0 °C

1.86E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.86E-5 1/K

Unlock all property charts

Melting point

1230 - 1480 °C

Show Material materials with Melting point of 1230 - 1480 °C

Typical for Austenitic Stainless Steel

Specific heat capacity

-100.0 °C

440 J/(kg·K)

Show Material materials with Specific heat capacity of 440 J/(kg·K)

20.0 °C

472 J/(kg·K)

Show Material materials with Specific heat capacity of 472 J/(kg·K)

100.0 °C

487 J/(kg·K)

Show Material materials with Specific heat capacity of 487 J/(kg·K)

200.0 °C

503 J/(kg·K)

Show Material materials with Specific heat capacity of 503 J/(kg·K)

300.0 °C

512 J/(kg·K)

Show Material materials with Specific heat capacity of 512 J/(kg·K)

400.0 °C

520 J/(kg·K)

Show Material materials with Specific heat capacity of 520 J/(kg·K)

500.0 °C

530 J/(kg·K)

Show Material materials with Specific heat capacity of 530 J/(kg·K)

600.0 °C

541 J/(kg·K)

Show Material materials with Specific heat capacity of 541 J/(kg·K)

700.0 °C

551 J/(kg·K)

Show Material materials with Specific heat capacity of 551 J/(kg·K)

800.0 °C

559 J/(kg·K)

Show Material materials with Specific heat capacity of 559 J/(kg·K)

900.0 °C

565 J/(kg·K)

Show Material materials with Specific heat capacity of 565 J/(kg·K)

1000.0 °C

571 J/(kg·K)

Show Material materials with Specific heat capacity of 571 J/(kg·K)

Unlock all property charts

Thermal conductivity

20.0 °C

11.5 W/(m·K)

Show Material materials with Thermal conductivity of 11.5 W/(m·K)

100.0 °C

13.1 W/(m·K)

Show Material materials with Thermal conductivity of 13.1 W/(m·K)

200.0 °C

14.8 W/(m·K)

Show Material materials with Thermal conductivity of 14.8 W/(m·K)

300.0 °C

16.4 W/(m·K)

Show Material materials with Thermal conductivity of 16.4 W/(m·K)

400.0 °C

18.1 W/(m·K)

Show Material materials with Thermal conductivity of 18.1 W/(m·K)

500.0 °C

19.6 W/(m·K)

Show Material materials with Thermal conductivity of 19.6 W/(m·K)

600.0 °C

21.2 W/(m·K)

Show Material materials with Thermal conductivity of 21.2 W/(m·K)

700.0 °C

22.8 W/(m·K)

Show Material materials with Thermal conductivity of 22.8 W/(m·K)

800.0 °C

24.3 W/(m·K)

Show Material materials with Thermal conductivity of 24.3 W/(m·K)

900.0 °C

25.7 W/(m·K)

Show Material materials with Thermal conductivity of 25.7 W/(m·K)

1000.0 °C

27.3 W/(m·K)

Show Material materials with Thermal conductivity of 27.3 W/(m·K)

Unlock all property charts

Thermal diffusivity

20.0 °C

3.1 mm²/s

Show Material materials with Thermal diffusivity of 3.1 mm²/s

100.0 °C

3.3 mm²/s

Show Material materials with Thermal diffusivity of 3.3 mm²/s

200.0 °C

3.6 mm²/s

Show Material materials with Thermal diffusivity of 3.6 mm²/s

300.0 °C

3.9 mm²/s

Show Material materials with Thermal diffusivity of 3.9 mm²/s

400.0 °C

4.2 mm²/s

Show Material materials with Thermal diffusivity of 4.2 mm²/s

500.0 °C

4.4 mm²/s

Show Material materials with Thermal diffusivity of 4.4 mm²/s

600.0 °C

4.6 mm²/s

Show Material materials with Thermal diffusivity of 4.6 mm²/s

700.0 °C

4.9 mm²/s

Show Material materials with Thermal diffusivity of 4.9 mm²/s

800.0 °C

5.2 mm²/s

Show Material materials with Thermal diffusivity of 5.2 mm²/s

900.0 °C

5.5 mm²/s

Show Material materials with Thermal diffusivity of 5.5 mm²/s

1000.0 °C

5.7 mm²/s

Show Material materials with Thermal diffusivity of 5.7 mm²/s

Unlock all property charts

Electrical

PropertyTemperatureValue

Electrical resistivity

20.0 °C

1.01E-6 Ω·m

Show Material materials with Electrical resistivity of 1.01E-6 Ω·m

100.0 °C

1.04E-6 Ω·m

Show Material materials with Electrical resistivity of 1.04E-6 Ω·m

200.0 °C

1.08E-6 Ω·m

Show Material materials with Electrical resistivity of 1.08E-6 Ω·m

300.0 °C

1.12E-6 Ω·m

Show Material materials with Electrical resistivity of 1.12E-6 Ω·m

400.0 °C

1.15E-6 Ω·m

Show Material materials with Electrical resistivity of 1.15E-6 Ω·m

500.0 °C

1.18E-6 Ω·m

Show Material materials with Electrical resistivity of 1.18E-6 Ω·m

600.0 °C

1.2E-6 Ω·m

Show Material materials with Electrical resistivity of 1.2E-6 Ω·m

700.0 °C

1.22E-6 Ω·m

Show Material materials with Electrical resistivity of 1.22E-6 Ω·m

800.0 °C

1.24E-6 Ω·m

Show Material materials with Electrical resistivity of 1.24E-6 Ω·m

900.0 °C

1.26E-6 Ω·m

Show Material materials with Electrical resistivity of 1.26E-6 Ω·m

1000.0 °C

1.27E-6 Ω·m

Show Material materials with Electrical resistivity of 1.27E-6 Ω·m

Unlock all property charts

Chemical properties

PropertyValue

Aluminium

0.2 - 0.5 %

Show Material materials with Aluminium of 0.2 - 0.5 %

Carbon

0.03 - 0.08 %

Show Material materials with Carbon of 0.03 - 0.08 %

Chromium

19 - 22 %

Show Material materials with Chromium of 19 - 22 %

Cobalt

0.5 %

Show Material materials with Cobalt of 0.5 %

Copper

0.5 %

Show Material materials with Copper of 0.5 %

Manganese

1.5 %

Show Material materials with Manganese of 1.5 %

Nickel

30 - 32.5 %

Show Material materials with Nickel of 30 - 32.5 %

Niobium

0.1 %

Show Material materials with Niobium of 0.1 %

Phosphorus

0.02 %

Show Material materials with Phosphorus of 0.02 %

Silicon

0.7 %

Show Material materials with Silicon of 0.7 %

Sulfur

0.01 %

Show Material materials with Sulfur of 0.01 %

Titanium

0.2 - 0.5 %