EN 10216-5 Grade X8CrNiMoNb16-16 solution annealed (+AT)

Want to keep this datasheet? Save it now in your required format

Description

Fully austenitic high temperature special steel which is resistant to scaling up to 750 degrees C and has a good creep resistance up to 700 degrees C. Used in steam and gas turbine construction (shovels, flanges, valves, nozzles, casings and bolts), for parts in the reactor technology and in the petrochemical industry.

Related Standards

Equivalent Materials

This material data has been provided by WIAM.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValue

Density

20.0 °C

8.01 g/cm³

Show Material materials with Density of 8.01 g/cm³

Mechanical

PropertyTemperatureValueComment

Elastic modulus

-100.0 °C

206 GPa

Show Material materials with Elastic modulus of 206 GPa

20.0 °C

196 GPa

Show Material materials with Elastic modulus of 196 GPa

100.0 °C

190 GPa

Show Material materials with Elastic modulus of 190 GPa

200.0 °C

182 GPa

Show Material materials with Elastic modulus of 182 GPa

300.0 °C

174 GPa

Show Material materials with Elastic modulus of 174 GPa

400.0 °C

166 GPa

Show Material materials with Elastic modulus of 166 GPa

500.0 °C

158 GPa

Show Material materials with Elastic modulus of 158 GPa

600.0 °C

150 GPa

Show Material materials with Elastic modulus of 150 GPa

700.0 °C

142 GPa

Show Material materials with Elastic modulus of 142 GPa

800.0 °C

134 GPa

Show Material materials with Elastic modulus of 134 GPa

Elongation

20.0 °C

35 %

Show Material materials with Elongation of 35 %

Elongation, transverse

20.0 °C

22 %

Show Material materials with Elongation, transverse of 22 %

Poisson's ratio

23.0 °C

0.3 [-]

Show Material materials with Poisson's ratio of 0.3 [-]

Typical for Austenitic Stainless Steel

Shear modulus

23.0 °C

77 GPa

Show Material materials with Shear modulus of 77 GPa

Typical for Austenitic Stainless Steel

Tensile strength

20.0 °C

530 - 690 MPa

Show Material materials with Tensile strength of 530 - 690 MPa

Tensile strength, transverse

20.0 °C

530 - 690 MPa

Show Material materials with Tensile strength, transverse of 530 - 690 MPa

Yield strength Rp0.2

20.0 °C

215 MPa

Show Material materials with Yield strength Rp0.2 of 215 MPa

100.0 °C

195 MPa

Show Material materials with Yield strength Rp0.2 of 195 MPa

200.0 °C

177 MPa

Show Material materials with Yield strength Rp0.2 of 177 MPa

300.0 °C

157 MPa

Show Material materials with Yield strength Rp0.2 of 157 MPa

400.0 °C

147 MPa

Show Material materials with Yield strength Rp0.2 of 147 MPa

500.0 °C

137 MPa

Show Material materials with Yield strength Rp0.2 of 137 MPa

550.0 °C

137 MPa

Show Material materials with Yield strength Rp0.2 of 137 MPa

600.0 °C

132 MPa

Show Material materials with Yield strength Rp0.2 of 132 MPa

Unlock all property charts

Yield strength Rp0.2, transverse

20.0 °C

215 MPa

Show Material materials with Yield strength Rp0.2, transverse of 215 MPa

Yield strength Rp1.0

20.0 °C

255 MPa

Show Material materials with Yield strength Rp1.0 of 255 MPa

100.0 °C

225 MPa

Show Material materials with Yield strength Rp1.0 of 225 MPa

200.0 °C

206 MPa

Show Material materials with Yield strength Rp1.0 of 206 MPa

300.0 °C

186 MPa

Show Material materials with Yield strength Rp1.0 of 186 MPa

400.0 °C

177 MPa

Show Material materials with Yield strength Rp1.0 of 177 MPa

500.0 °C

167 MPa

Show Material materials with Yield strength Rp1.0 of 167 MPa

550.0 °C

167 MPa

Show Material materials with Yield strength Rp1.0 of 167 MPa

600.0 °C

162 MPa

Show Material materials with Yield strength Rp1.0 of 162 MPa

Unlock all property charts

Yield strength Rp1.0, transverse

20.0 °C

255 MPa

Show Material materials with Yield strength Rp1.0, transverse of 255 MPa

Thermal

PropertyTemperatureValueComment

Coefficient of thermal expansion

-100.0 °C

1.49E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.49E-5 1/K

20.0 °C

1.61E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.61E-5 1/K

100.0 °C

1.67E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.67E-5 1/K

200.0 °C

1.72E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.72E-5 1/K

300.0 °C

1.77E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.77E-5 1/K

400.0 °C

1.81E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.81E-5 1/K

500.0 °C

1.84E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.84E-5 1/K

600.0 °C

1.88E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.88E-5 1/K

700.0 °C

1.91E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.91E-5 1/K

800.0 °C

1.94E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.94E-5 1/K

900.0 °C

1.97E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.97E-5 1/K

1000.0 °C

2E-5 1/K

Show Material materials with Coefficient of thermal expansion of 2E-5 1/K

Unlock all property charts

Melting point

1230 - 1480 °C

Show Material materials with Melting point of 1230 - 1480 °C

Typical for Austenitic Stainless Steel

Specific heat capacity

-100.0 °C

440 J/(kg·K)

Show Material materials with Specific heat capacity of 440 J/(kg·K)

20.0 °C

472 J/(kg·K)

Show Material materials with Specific heat capacity of 472 J/(kg·K)

100.0 °C

487 J/(kg·K)

Show Material materials with Specific heat capacity of 487 J/(kg·K)

200.0 °C

503 J/(kg·K)

Show Material materials with Specific heat capacity of 503 J/(kg·K)

300.0 °C

512 J/(kg·K)

Show Material materials with Specific heat capacity of 512 J/(kg·K)

400.0 °C

520 J/(kg·K)

Show Material materials with Specific heat capacity of 520 J/(kg·K)

500.0 °C

530 J/(kg·K)

Show Material materials with Specific heat capacity of 530 J/(kg·K)

600.0 °C

541 J/(kg·K)

Show Material materials with Specific heat capacity of 541 J/(kg·K)

700.0 °C

551 J/(kg·K)

Show Material materials with Specific heat capacity of 551 J/(kg·K)

800.0 °C

559 J/(kg·K)

Show Material materials with Specific heat capacity of 559 J/(kg·K)

900.0 °C

565 J/(kg·K)

Show Material materials with Specific heat capacity of 565 J/(kg·K)

1000.0 °C

571 J/(kg·K)

Show Material materials with Specific heat capacity of 571 J/(kg·K)

Unlock all property charts

Thermal conductivity

20.0 °C

13.5 W/(m·K)

Show Material materials with Thermal conductivity of 13.5 W/(m·K)

100.0 °C

14.9 W/(m·K)

Show Material materials with Thermal conductivity of 14.9 W/(m·K)

200.0 °C

16.7 W/(m·K)

Show Material materials with Thermal conductivity of 16.7 W/(m·K)

300.0 °C

18.3 W/(m·K)

Show Material materials with Thermal conductivity of 18.3 W/(m·K)

400.0 °C

19.8 W/(m·K)

Show Material materials with Thermal conductivity of 19.8 W/(m·K)

500.0 °C

21.3 W/(m·K)

Show Material materials with Thermal conductivity of 21.3 W/(m·K)

600.0 °C

22.7 W/(m·K)

Show Material materials with Thermal conductivity of 22.7 W/(m·K)

700.0 °C

24.2 W/(m·K)

Show Material materials with Thermal conductivity of 24.2 W/(m·K)

800.0 °C

25.6 W/(m·K)

Show Material materials with Thermal conductivity of 25.6 W/(m·K)

Unlock all property charts

Thermal diffusivity

20.0 °C

3.6 mm²/s

Show Material materials with Thermal diffusivity of 3.6 mm²/s

100.0 °C

3.7 mm²/s

Show Material materials with Thermal diffusivity of 3.7 mm²/s

200.0 °C

4 mm²/s

Show Material materials with Thermal diffusivity of 4 mm²/s

300.0 °C

4.4 mm²/s

Show Material materials with Thermal diffusivity of 4.4 mm²/s

400.0 °C

4.6 mm²/s

Show Material materials with Thermal diffusivity of 4.6 mm²/s

500.0 °C

4.7 mm²/s

Show Material materials with Thermal diffusivity of 4.7 mm²/s

600.0 °C

4.9 mm²/s

Show Material materials with Thermal diffusivity of 4.9 mm²/s

700.0 °C

5.2 mm²/s

Show Material materials with Thermal diffusivity of 5.2 mm²/s

800.0 °C

5.5 mm²/s

Show Material materials with Thermal diffusivity of 5.5 mm²/s

Unlock all property charts

Electrical

PropertyTemperatureValue

Electrical resistivity

20.0 °C

7.75E-7 Ω·m

Show Material materials with Electrical resistivity of 7.75E-7 Ω·m

100.0 °C

8.42E-7 Ω·m

Show Material materials with Electrical resistivity of 8.42E-7 Ω·m

200.0 °C

9.04E-7 Ω·m

Show Material materials with Electrical resistivity of 9.04E-7 Ω·m

300.0 °C

9.62E-7 Ω·m

Show Material materials with Electrical resistivity of 9.62E-7 Ω·m

400.0 °C

1.01E-6 Ω·m

Show Material materials with Electrical resistivity of 1.01E-6 Ω·m

500.0 °C

1.06E-6 Ω·m

Show Material materials with Electrical resistivity of 1.06E-6 Ω·m

600.0 °C

1.1E-6 Ω·m

Show Material materials with Electrical resistivity of 1.1E-6 Ω·m

700.0 °C

1.13E-6 Ω·m

Show Material materials with Electrical resistivity of 1.13E-6 Ω·m

800.0 °C

1.16E-6 Ω·m

Show Material materials with Electrical resistivity of 1.16E-6 Ω·m

Unlock all property charts

Chemical properties

PropertyValue

Carbon

0.04 - 0.1 %

Show Material materials with Carbon of 0.04 - 0.1 %

Chromium

15.5 - 17.5 %

Show Material materials with Chromium of 15.5 - 17.5 %

Manganese

1.5 %

Show Material materials with Manganese of 1.5 %

Molybdenum

1.6 - 2 %

Show Material materials with Molybdenum of 1.6 - 2 %

Nickel

15.5 - 17.5 %

Show Material materials with Nickel of 15.5 - 17.5 %

Niobium

1.2 %

Show Material materials with Niobium of 1.2 %

Phosphorus

0.04 %

Show Material materials with Phosphorus of 0.04 %

Silicon

0.3 - 0.6 %

Show Material materials with Silicon of 0.3 - 0.6 %

Sulfur

0.015 %

Show Material materials with Sulfur of 0.015 %