DIN 17480 Grade NiFe25Cr20NbTi solution heat-treated and precipitation hardened (+AT+P)

Want to keep this datasheet? Save it now in your required format

Related Standards

Equivalent Materials

This material data has been provided by WIAM.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValue

Density

20.0 °C

8.1 g/cm³

Show Material materials with Density of 8.1 g/cm³

Mechanical

PropertyTemperatureValueComment

Elastic modulus

20.0 °C

215 GPa

Show Material materials with Elastic modulus of 215 GPa

Elongation

20.0 °C

25 %

Show Material materials with Elongation of 25 %

Hardness, Rockwell C

20.0 °C

28 [-]

Show Material materials with Hardness, Rockwell C of 28 [-]

Poisson's ratio

23.0 °C

0.29 [-]

Show Material materials with Poisson's ratio of 0.29 [-]

Typical for Nickel Steel

Reduction of area

20.0 °C

30 %

Show Material materials with Reduction of area of 30 %

Shear modulus

23.0 °C

76 GPa

Show Material materials with Shear modulus of 76 GPa

Typical for Nickel Steel

Tensile strength

20.0 °C

900 - 1100 MPa

Show Material materials with Tensile strength of 900 - 1100 MPa

500.0 °C

800 MPa

Show Material materials with Tensile strength of 800 MPa

550.0 °C

800 MPa

Show Material materials with Tensile strength of 800 MPa

600.0 °C

790 MPa

Show Material materials with Tensile strength of 790 MPa

650.0 °C

740 MPa

Show Material materials with Tensile strength of 740 MPa

700.0 °C

640 MPa

Show Material materials with Tensile strength of 640 MPa

750.0 °C

500 MPa

Show Material materials with Tensile strength of 500 MPa

800.0 °C

340 MPa

Show Material materials with Tensile strength of 340 MPa

Yield strength Rp0.2

20.0 °C

500 MPa

Show Material materials with Yield strength Rp0.2 of 500 MPa

500.0 °C

450 MPa

Show Material materials with Yield strength Rp0.2 of 450 MPa

550.0 °C

450 MPa

Show Material materials with Yield strength Rp0.2 of 450 MPa

600.0 °C

450 MPa

Show Material materials with Yield strength Rp0.2 of 450 MPa

650.0 °C

430 MPa

Show Material materials with Yield strength Rp0.2 of 430 MPa

700.0 °C

430 MPa

Show Material materials with Yield strength Rp0.2 of 430 MPa

750.0 °C

380 MPa

Show Material materials with Yield strength Rp0.2 of 380 MPa

800.0 °C

250 MPa

Show Material materials with Yield strength Rp0.2 of 250 MPa

Unlock all property charts

Thermal

PropertyTemperatureValueComment

Coefficient of thermal expansion

100.0 °C

1.41E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.41E-5 1/K

300.0 °C

1.55E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.55E-5 1/K

500.0 °C

1.59E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.59E-5 1/K

700.0 °C

1.68E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.68E-5 1/K

Unlock all property charts

Max service temperature, long

0 - 700 °C

Show Material materials with Max service temperature, long of 0 - 700 °C

Melting point

1316 - 1595 °C

Show Material materials with Melting point of 1316 - 1595 °C

Typical for Nickel Steel

Specific heat capacity

20.0 °C

460 J/(kg·K)

Show Material materials with Specific heat capacity of 460 J/(kg·K)

Thermal conductivity

20.0 °C

13 W/(m·K)

Show Material materials with Thermal conductivity of 13 W/(m·K)

Chemical properties

PropertyValue

Aluminium

0.3 - 1 %

Show Material materials with Aluminium of 0.3 - 1 %

Boron

8E-3 %

Show Material materials with Boron of 8E-3 %

Carbon

0.1 %

Show Material materials with Carbon of 0.1 %

Chromium

18 - 21 %

Show Material materials with Chromium of 18 - 21 %

Iron

23 - 28 %

Show Material materials with Iron of 23 - 28 %

Manganese

1 %

Show Material materials with Manganese of 1 %

Phosphorus

0.03 %

Show Material materials with Phosphorus of 0.03 %

Silicon

1 %

Show Material materials with Silicon of 1 %

Sulfur

0.015 %

Show Material materials with Sulfur of 0.015 %

Titanium

1 - 2 %

Show Material materials with Titanium of 1 - 2 %