General
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Density | 20 °C | 7.85 g/cm³ Show Material materials with Density of 7.85 g/cm³ | normalized or normalized formed (+N) | EN 10025, DIN 5512-1 | Sheet, Strip, Flat, Wire, Bar |
Mechanical
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Elastic modulus | -100 °C | 217 GPa Show Material materials with Elastic modulus of 217 GPa | normalized or normalized formed (+N) | EN 10025, DIN 5512-1 | Sheet, Strip, Flat, Wire, Bar | |
20 °C | 212 GPa Show Material materials with Elastic modulus of 212 GPa | normalized or normalized formed (+N) | EN 10025, DIN 5512-1 | Sheet, Strip, Flat, Wire, Bar | ||
100 °C | 207 GPa Show Material materials with Elastic modulus of 207 GPa | normalized or normalized formed (+N) | EN 10025, DIN 5512-1 | Sheet, Strip, Flat, Wire, Bar | ||
200 °C | 199 GPa Show Material materials with Elastic modulus of 199 GPa | normalized or normalized formed (+N) | EN 10025, DIN 5512-1 | Sheet, Strip, Flat, Wire, Bar | ||
300 °C | 192 GPa Show Material materials with Elastic modulus of 192 GPa | normalized or normalized formed (+N) | EN 10025, DIN 5512-1 | Sheet, Strip, Flat, Wire, Bar | ||
400 °C | 184 GPa Show Material materials with Elastic modulus of 184 GPa | normalized or normalized formed (+N) | EN 10025, DIN 5512-1 | Sheet, Strip, Flat, Wire, Bar | ||
500 °C | 175 GPa Show Material materials with Elastic modulus of 175 GPa | normalized or normalized formed (+N) | EN 10025, DIN 5512-1 | Sheet, Strip, Flat, Wire, Bar | ||
600 °C | 164 GPa Show Material materials with Elastic modulus of 164 GPa | normalized or normalized formed (+N) | EN 10025, DIN 5512-1 | Sheet, Strip, Flat, Wire, Bar | ||
Elongation | 20 °C | 15 % Show Material materials with Elongation of 15 % | normalized or normalized formed (+N) | EN 10025, DIN 5512-1 | Sheet, Strip, Flat | A80 Transverse |
20 °C | 16 % Show Material materials with Elongation of 16 % | normalized or normalized formed (+N) | EN 10025, DIN 5512-1 | Sheet, Strip, Flat | A80 Transverse | |
20 °C | 17 % Show Material materials with Elongation of 17 % | normalized or normalized formed (+N) | EN 10025, DIN 5512-1 | Sheet, Strip, Flat | A80 Transverse | |
20 °C | 17 % Show Material materials with Elongation of 17 % | normalized or normalized formed (+N) | EN 10025, DIN 5512-1 | Sheet, Strip, Flat, Wire | A80 | |
20 °C | 18 % Show Material materials with Elongation of 18 % | normalized or normalized formed (+N) | EN 10025, DIN 5512-1 | Sheet, Strip, Flat | A80 Transverse | |
20 °C | 18 % Show Material materials with Elongation of 18 % | normalized or normalized formed (+N) | EN 10025, DIN 5512-1 | Sheet, Strip, Flat, Wire | A80 | |
20 °C | 19 % Show Material materials with Elongation of 19 % | normalized or normalized formed (+N) | EN 10025, DIN 5512-1 | Sheet, Strip, Flat | A80 Transverse | |
20 °C | 19 % Show Material materials with Elongation of 19 % | normalized or normalized formed (+N) | EN 10025, DIN 5512-1 | Sheet, Strip, Flat, Wire | A80 | |
20 °C | 20 % Show Material materials with Elongation of 20 % | normalized or normalized formed (+N) | EN 10025, DIN 5512-1 | Sheet, Strip, Flat, Wire | A80 | |
20 °C | 21 % Show Material materials with Elongation of 21 % | normalized or normalized formed (+N) | EN 10025, DIN 5512-1 | Sheet, Strip, Flat | Transverse | |
20 °C | 21 % Show Material materials with Elongation of 21 % | normalized or normalized formed (+N) | EN 10025, DIN 5512-1 | Sheet, Flat, Bar | ||
20 °C | 21 % Show Material materials with Elongation of 21 % | normalized or normalized formed (+N) | EN 10025, DIN 5512-1 | Sheet, Strip, Flat, Wire | A80 | |
20 °C | 22 % Show Material materials with Elongation of 22 % | normalized or normalized formed (+N) | EN 10025, DIN 5512-1 | Sheet, Strip, Flat | Transverse | |
20 °C | 22 % Show Material materials with Elongation of 22 % | normalized or normalized formed (+N) | EN 10025, DIN 5512-1 | Sheet, Flat, Bar | ||
20 °C | 23 % Show Material materials with Elongation of 23 % | normalized or normalized formed (+N) | EN 10025, DIN 5512-1 | Sheet, Strip, Flat | Transverse | |
20 °C | 24 % Show Material materials with Elongation of 24 % | normalized or normalized formed (+N) | EN 10025, DIN 5512-1 | Sheet, Strip, Flat | Transverse | |
20 °C | 24 % Show Material materials with Elongation of 24 % | normalized or normalized formed (+N) | EN 10025, DIN 5512-1 | Sheet, Flat, Bar | ||
20 °C | 25 % Show Material materials with Elongation of 25 % | normalized or normalized formed (+N) | EN 10025, DIN 5512-1 | Sheet, Strip, Flat | ||
20 °C | 26 % Show Material materials with Elongation of 26 % | normalized or normalized formed (+N) | EN 10025, DIN 5512-1 | Sheet, Strip, Flat, Wire | ||
Poisson's ratio | 20 °C | 0.284 [-] Show Material materials with Poisson's ratio of 0.284 [-] | normalized or normalized formed (+N) | EN 10025, DIN 5512-1 | Sheet, Strip, Flat, Wire, Bar | |
Shear modulus | 82 GPa Show Material materials with Shear modulus of 82 GPa | Typical for Low Carbon Steel | ||||
Tensile strength | 20 °C | 320 - 470 MPa Show Material materials with Tensile strength of 320 - 470 MPa | normalized or normalized formed (+N) | EN 10025, DIN 5512-1 | Sheet, Flat, Bar | |
20 °C | 340 - 470 MPa Show Material materials with Tensile strength of 340 - 470 MPa | normalized or normalized formed (+N) | EN 10025, DIN 5512-1 | Sheet, Strip, Flat, Wire, Bar | ||
20 °C | 340 - 510 MPa Show Material materials with Tensile strength of 340 - 510 MPa | normalized or normalized formed (+N) | EN 10025, DIN 5512-1 | Sheet, Strip, Flat, Wire | ||
20 °C | 360 - 510 MPa Show Material materials with Tensile strength of 360 - 510 MPa | normalized or normalized formed (+N) | EN 10025, DIN 5512-1 | Sheet, Strip, Flat, Wire | ||
20 °C | 360 - 470 MPa Show Material materials with Tensile strength of 360 - 470 MPa | normalized or normalized formed (+N) | EN 10025, DIN 5512-1 | Sheet, Strip, Flat, Wire | ||
Yield strength | 20 °C | 175 MPa Show Material materials with Yield strength of 175 MPa | normalized or normalized formed (+N) | EN 10025, DIN 5512-1 | Sheet, Flat, Bar | |
20 °C | 185 MPa Show Material materials with Yield strength of 185 MPa | normalized or normalized formed (+N) | EN 10025, DIN 5512-1 | Sheet, Flat, Bar | ||
20 °C | 195 MPa Show Material materials with Yield strength of 195 MPa | normalized or normalized formed (+N) | EN 10025, DIN 5512-1 | Sheet, Flat, Bar | ||
20 °C | 215 MPa Show Material materials with Yield strength of 215 MPa | normalized or normalized formed (+N) | EN 10025, DIN 5512-1 | Sheet, Strip, Flat, Bar | ||
20 °C | 225 MPa Show Material materials with Yield strength of 225 MPa | normalized or normalized formed (+N) | EN 10025, DIN 5512-1 | Sheet, Strip, Flat | ||
20 °C | 235 MPa Show Material materials with Yield strength of 235 MPa | normalized or normalized formed (+N) | EN 10025, DIN 5512-1 | Sheet, Strip, Flat, Wire |
Thermal
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Coefficient of thermal expansion | -100 °C | 1.08e-05 1/K Show Material materials with Coefficient of thermal expansion of 1.08e-05 1/K | normalized or normalized formed (+N) | EN 10025, DIN 5512-1 | Sheet, Strip, Flat, Wire, Bar | |
20 °C | 1.19e-05 1/K Show Material materials with Coefficient of thermal expansion of 1.19e-05 1/K | normalized or normalized formed (+N) | EN 10025, DIN 5512-1 | Sheet, Strip, Flat, Wire, Bar | ||
100 °C | 1.25e-05 1/K Show Material materials with Coefficient of thermal expansion of 1.25e-05 1/K | normalized or normalized formed (+N) | EN 10025, DIN 5512-1 | Sheet, Strip, Flat, Wire, Bar | ||
200 °C | 1.3e-05 1/K Show Material materials with Coefficient of thermal expansion of 1.3e-05 1/K | normalized or normalized formed (+N) | EN 10025, DIN 5512-1 | Sheet, Strip, Flat, Wire, Bar | ||
300 °C | 1.36e-05 1/K Show Material materials with Coefficient of thermal expansion of 1.36e-05 1/K | normalized or normalized formed (+N) | EN 10025, DIN 5512-1 | Sheet, Strip, Flat, Wire, Bar | ||
400 °C | 1.41e-05 1/K Show Material materials with Coefficient of thermal expansion of 1.41e-05 1/K | normalized or normalized formed (+N) | EN 10025, DIN 5512-1 | Sheet, Strip, Flat, Wire, Bar | ||
500 °C | 1.45e-05 1/K Show Material materials with Coefficient of thermal expansion of 1.45e-05 1/K | normalized or normalized formed (+N) | EN 10025, DIN 5512-1 | Sheet, Strip, Flat, Wire, Bar | ||
600 °C | 1.49e-05 1/K Show Material materials with Coefficient of thermal expansion of 1.49e-05 1/K | normalized or normalized formed (+N) | EN 10025, DIN 5512-1 | Sheet, Strip, Flat, Wire, Bar | ||
Max service temperature | 500 °C Show Material materials with Max service temperature of 500 °C | Typical for Carbon Steel | ||||
Melting point | 1480 - 1526 °C Show Material materials with Melting point of 1480 - 1526 °C | Typical for Low Carbon Steel | ||||
Specific heat capacity | -100 °C | 423 J/(kg·K) Show Material materials with Specific heat capacity of 423 J/(kg·K) | normalized or normalized formed (+N) | EN 10025, DIN 5512-1 | Sheet, Strip, Flat, Wire, Bar | |
20 °C | 461 J/(kg·K) Show Material materials with Specific heat capacity of 461 J/(kg·K) | normalized or normalized formed (+N) | EN 10025, DIN 5512-1 | Sheet, Strip, Flat, Wire, Bar | ||
100 °C | 479 J/(kg·K) Show Material materials with Specific heat capacity of 479 J/(kg·K) | normalized or normalized formed (+N) | EN 10025, DIN 5512-1 | Sheet, Strip, Flat, Wire, Bar | ||
200 °C | 499 J/(kg·K) Show Material materials with Specific heat capacity of 499 J/(kg·K) | normalized or normalized formed (+N) | EN 10025, DIN 5512-1 | Sheet, Strip, Flat, Wire, Bar | ||
300 °C | 517 J/(kg·K) Show Material materials with Specific heat capacity of 517 J/(kg·K) | normalized or normalized formed (+N) | EN 10025, DIN 5512-1 | Sheet, Strip, Flat, Wire, Bar | ||
400 °C | 536 J/(kg·K) Show Material materials with Specific heat capacity of 536 J/(kg·K) | normalized or normalized formed (+N) | EN 10025, DIN 5512-1 | Sheet, Strip, Flat, Wire, Bar | ||
500 °C | 558 J/(kg·K) Show Material materials with Specific heat capacity of 558 J/(kg·K) | normalized or normalized formed (+N) | EN 10025, DIN 5512-1 | Sheet, Strip, Flat, Wire, Bar | ||
600 °C | 587 J/(kg·K) Show Material materials with Specific heat capacity of 587 J/(kg·K) | normalized or normalized formed (+N) | EN 10025, DIN 5512-1 | Sheet, Strip, Flat, Wire, Bar | ||
Thermal conductivity | 20 °C | 56.9 W/(m·K) Show Material materials with Thermal conductivity of 56.9 W/(m·K) | normalized or normalized formed (+N) | EN 10025, DIN 5512-1 | Sheet, Strip, Flat, Wire, Bar | |
100 °C | 56.4 W/(m·K) Show Material materials with Thermal conductivity of 56.4 W/(m·K) | normalized or normalized formed (+N) | EN 10025, DIN 5512-1 | Sheet, Strip, Flat, Wire, Bar | ||
200 °C | 53.5 W/(m·K) Show Material materials with Thermal conductivity of 53.5 W/(m·K) | normalized or normalized formed (+N) | EN 10025, DIN 5512-1 | Sheet, Strip, Flat, Wire, Bar | ||
300 °C | 49.4 W/(m·K) Show Material materials with Thermal conductivity of 49.4 W/(m·K) | normalized or normalized formed (+N) | EN 10025, DIN 5512-1 | Sheet, Strip, Flat, Wire, Bar | ||
400 °C | 45.2 W/(m·K) Show Material materials with Thermal conductivity of 45.2 W/(m·K) | normalized or normalized formed (+N) | EN 10025, DIN 5512-1 | Sheet, Strip, Flat, Wire, Bar | ||
500 °C | 41.3 W/(m·K) Show Material materials with Thermal conductivity of 41.3 W/(m·K) | normalized or normalized formed (+N) | EN 10025, DIN 5512-1 | Sheet, Strip, Flat, Wire, Bar | ||
600 °C | 37.6 W/(m·K) Show Material materials with Thermal conductivity of 37.6 W/(m·K) | normalized or normalized formed (+N) | EN 10025, DIN 5512-1 | Sheet, Strip, Flat, Wire, Bar | ||
Thermal diffusivity | 20 °C | 15.7 mm²/s Show Material materials with Thermal diffusivity of 15.7 mm²/s | normalized or normalized formed (+N) | EN 10025, DIN 5512-1 | Sheet, Strip, Flat, Wire, Bar | |
100 °C | 14.5 mm²/s Show Material materials with Thermal diffusivity of 14.5 mm²/s | normalized or normalized formed (+N) | EN 10025, DIN 5512-1 | Sheet, Strip, Flat, Wire, Bar | ||
200 °C | 12.9 mm²/s Show Material materials with Thermal diffusivity of 12.9 mm²/s | normalized or normalized formed (+N) | EN 10025, DIN 5512-1 | Sheet, Strip, Flat, Wire, Bar | ||
300 °C | 11.2 mm²/s Show Material materials with Thermal diffusivity of 11.2 mm²/s | normalized or normalized formed (+N) | EN 10025, DIN 5512-1 | Sheet, Strip, Flat, Wire, Bar | ||
400 °C | 9.6 mm²/s Show Material materials with Thermal diffusivity of 9.6 mm²/s | normalized or normalized formed (+N) | EN 10025, DIN 5512-1 | Sheet, Strip, Flat, Wire, Bar | ||
500 °C | 7.9 mm²/s Show Material materials with Thermal diffusivity of 7.9 mm²/s | normalized or normalized formed (+N) | EN 10025, DIN 5512-1 | Sheet, Strip, Flat, Wire, Bar | ||
600 °C | 6.3 mm²/s Show Material materials with Thermal diffusivity of 6.3 mm²/s | normalized or normalized formed (+N) | EN 10025, DIN 5512-1 | Sheet, Strip, Flat, Wire, Bar |
Electrical
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Electrical resistivity | 20 °C | 1.83e-07 Ω·m Show Material materials with Electrical resistivity of 1.83e-07 Ω·m | normalized or normalized formed (+N) | EN 10025, DIN 5512-1 | Sheet, Strip, Flat, Wire, Bar |
100 °C | 2.27e-07 Ω·m Show Material materials with Electrical resistivity of 2.27e-07 Ω·m | normalized or normalized formed (+N) | EN 10025, DIN 5512-1 | Sheet, Strip, Flat, Wire, Bar | |
200 °C | 2.95e-07 Ω·m Show Material materials with Electrical resistivity of 2.95e-07 Ω·m | normalized or normalized formed (+N) | EN 10025, DIN 5512-1 | Sheet, Strip, Flat, Wire, Bar | |
300 °C | 3.8e-07 Ω·m Show Material materials with Electrical resistivity of 3.8e-07 Ω·m | normalized or normalized formed (+N) | EN 10025, DIN 5512-1 | Sheet, Strip, Flat, Wire, Bar | |
400 °C | 4.81e-07 Ω·m Show Material materials with Electrical resistivity of 4.81e-07 Ω·m | normalized or normalized formed (+N) | EN 10025, DIN 5512-1 | Sheet, Strip, Flat, Wire, Bar | |
500 °C | 5.99e-07 Ω·m Show Material materials with Electrical resistivity of 5.99e-07 Ω·m | normalized or normalized formed (+N) | EN 10025, DIN 5512-1 | Sheet, Strip, Flat, Wire, Bar | |
600 °C | 7.38e-07 Ω·m Show Material materials with Electrical resistivity of 7.38e-07 Ω·m | normalized or normalized formed (+N) | EN 10025, DIN 5512-1 | Sheet, Strip, Flat, Wire, Bar |
Magnetic
Property | Value | Comment |
---|---|---|
Curie temperature | 770 °C Show Material materials with Curie temperature of 770 °C | Typical for Low Carbon Steel |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Carbon | 0.17 Show Material materials with Carbon of 0.17 | normalized or normalized formed (+N) | EN 10025, DIN 5512-1 | Sheet, Strip, Flat, Wire, Bar |
Manganese | 1.4 Show Material materials with Manganese of 1.4 | normalized or normalized formed (+N) | EN 10025, DIN 5512-1 | Sheet, Strip, Flat, Wire, Bar |
Phosphorus | 0.035 Show Material materials with Phosphorus of 0.035 | normalized or normalized formed (+N) | EN 10025, DIN 5512-1 | Sheet, Strip, Flat, Wire, Bar |
Sulfur | 0.035 Show Material materials with Sulfur of 0.035 | normalized or normalized formed (+N) | EN 10025, DIN 5512-1 | Sheet, Strip, Flat, Wire, Bar |