General
Property | Temperature | Value |
---|---|---|
Density | 20.0 °C | 7.85 g/cm³ Show Material materials with Density of 7.85 g/cm³ |
Mechanical
Property | Temperature | Value | Comment |
---|---|---|---|
Elastic modulus | 20.0 °C | 210 GPa Show Material materials with Elastic modulus of 210 GPa | |
100.0 °C | 205 GPa Show Material materials with Elastic modulus of 205 GPa | ||
200.0 °C | 195 GPa Show Material materials with Elastic modulus of 195 GPa | ||
300.0 °C | 185 GPa Show Material materials with Elastic modulus of 185 GPa | ||
400.0 °C | 175 GPa Show Material materials with Elastic modulus of 175 GPa | ||
Elongation | 20.0 °C | 22 % Show Material materials with Elongation of 22 % | |
Elongation A80 | 20.0 °C | 14 - 18 % Show Material materials with Elongation A80 of 14 - 18 % | |
Elongation A80, transverse | 20.0 °C | 12 - 16 % Show Material materials with Elongation A80, transverse of 12 - 16 % | |
Elongation, transverse | 20.0 °C | 20 % Show Material materials with Elongation, transverse of 20 % | |
Poisson's ratio | 23.0 °C | 0.29 [-] Show Material materials with Poisson's ratio of 0.29 [-] | Typical for Low Carbon Steel |
Shear modulus | 20.0 °C | 81 GPa Show Material materials with Shear modulus of 81 GPa | |
Tensile strength | 20.0 °C | 490 - 680 MPa Show Material materials with Tensile strength of 490 - 680 MPa | |
Yield strength | 20.0 °C | 345 - 355 MPa Show Material materials with Yield strength of 345 - 355 MPa |
Thermal
Property | Temperature | Value | Comment |
---|---|---|---|
Coefficient of thermal expansion | 100.0 °C | 1.11E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.11E-5 1/K | |
200.0 °C | 1.21E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.21E-5 1/K | ||
300.0 °C | 1.29E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.29E-5 1/K | ||
400.0 °C | 1.35E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.35E-5 1/K | ||
Max service temperature | 500 °C Show Material materials with Max service temperature of 500 °C | Typical for Carbon Steel | |
Melting point | 1480 - 1526 °C Show Material materials with Melting point of 1480 - 1526 °C | Typical for Low Carbon Steel | |
Specific heat capacity | 20.0 °C | 450 J/(kg·K) Show Material materials with Specific heat capacity of 450 J/(kg·K) | |
Thermal conductivity | 20.0 °C | 54 W/(m·K) Show Material materials with Thermal conductivity of 54 W/(m·K) | |
100.0 °C | 50.7 W/(m·K) Show Material materials with Thermal conductivity of 50.7 W/(m·K) | ||
200.0 °C | 46.9 W/(m·K) Show Material materials with Thermal conductivity of 46.9 W/(m·K) | ||
300.0 °C | 41.5 W/(m·K) Show Material materials with Thermal conductivity of 41.5 W/(m·K) | ||
400.0 °C | 39.4 W/(m·K) Show Material materials with Thermal conductivity of 39.4 W/(m·K) | ||
Electrical
Property | Temperature | Value |
---|---|---|
Electrical resistivity | 20.0 °C | 2E-7 Ω·m Show Material materials with Electrical resistivity of 2E-7 Ω·m |
Magnetic
Property | Value | Comment |
---|---|---|
Curie temperature | 770 °C Show Material materials with Curie temperature of 770 °C | Typical for Low Carbon Steel |
Chemical properties
Property | Value |
---|---|
Carbon | 0.2 % Show Material materials with Carbon of 0.2 % |
Manganese | 1.6 % Show Material materials with Manganese of 1.6 % |
Phosphorus | 0.04 % Show Material materials with Phosphorus of 0.04 % |
Silicon | 0.55 % Show Material materials with Silicon of 0.55 % |
Sulfur | 0.035 % Show Material materials with Sulfur of 0.035 % |