General
Property | Temperature | Value |
---|---|---|
Density | 20.0 °C | 7.83 g/cm³ Show Material materials with Density of 7.83 g/cm³ |
Mechanical
Property | Temperature | Value | Comment |
---|---|---|---|
Elastic modulus | -100.0 °C | 217 GPa Show Material materials with Elastic modulus of 217 GPa | |
20.0 °C | 212 GPa Show Material materials with Elastic modulus of 212 GPa | ||
100.0 °C | 207 GPa Show Material materials with Elastic modulus of 207 GPa | ||
200.0 °C | 199 GPa Show Material materials with Elastic modulus of 199 GPa | ||
300.0 °C | 192 GPa Show Material materials with Elastic modulus of 192 GPa | ||
400.0 °C | 184 GPa Show Material materials with Elastic modulus of 184 GPa | ||
500.0 °C | 175 GPa Show Material materials with Elastic modulus of 175 GPa | ||
600.0 °C | 164 GPa Show Material materials with Elastic modulus of 164 GPa | ||
Hardness, Brinell | 20.0 °C | 207 [-] Show Material materials with Hardness, Brinell of 207 [-] | |
Poisson's ratio | 23.0 °C | 0.29 [-] Show Material materials with Poisson's ratio of 0.29 [-] | Typical for Chromium Molybdenum Steel |
Thermal
Property | Temperature | Value | Comment |
---|---|---|---|
Coefficient of thermal expansion | -100.0 °C | 1.05E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.05E-5 1/K | |
20.0 °C | 1.15E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.15E-5 1/K | ||
100.0 °C | 1.21E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.21E-5 1/K | ||
200.0 °C | 1.27E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.27E-5 1/K | ||
300.0 °C | 1.32E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.32E-5 1/K | ||
400.0 °C | 1.36E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.36E-5 1/K | ||
500.0 °C | 1.4E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.4E-5 1/K | ||
600.0 °C | 1.44E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.44E-5 1/K | ||
Max service temperature, long | -60 - 0 °C Show Material materials with Max service temperature, long of -60 - 0 °C | ||
Melting point | 1382 - 1529 °C Show Material materials with Melting point of 1382 - 1529 °C | Typical for Chromium Molybdenum Steel | |
Specific heat capacity | -100.0 °C | 423 J/(kg·K) Show Material materials with Specific heat capacity of 423 J/(kg·K) | |
20.0 °C | 461 J/(kg·K) Show Material materials with Specific heat capacity of 461 J/(kg·K) | ||
100.0 °C | 479 J/(kg·K) Show Material materials with Specific heat capacity of 479 J/(kg·K) | ||
200.0 °C | 499 J/(kg·K) Show Material materials with Specific heat capacity of 499 J/(kg·K) | ||
300.0 °C | 517 J/(kg·K) Show Material materials with Specific heat capacity of 517 J/(kg·K) | ||
400.0 °C | 536 J/(kg·K) Show Material materials with Specific heat capacity of 536 J/(kg·K) | ||
500.0 °C | 558 J/(kg·K) Show Material materials with Specific heat capacity of 558 J/(kg·K) | ||
600.0 °C | 587 J/(kg·K) Show Material materials with Specific heat capacity of 587 J/(kg·K) | ||
Thermal conductivity | 20.0 °C | 41 W/(m·K) Show Material materials with Thermal conductivity of 41 W/(m·K) | |
100.0 °C | 42.7 W/(m·K) Show Material materials with Thermal conductivity of 42.7 W/(m·K) | ||
200.0 °C | 42.8 W/(m·K) Show Material materials with Thermal conductivity of 42.8 W/(m·K) | ||
300.0 °C | 41.6 W/(m·K) Show Material materials with Thermal conductivity of 41.6 W/(m·K) | ||
400.0 °C | 39.9 W/(m·K) Show Material materials with Thermal conductivity of 39.9 W/(m·K) | ||
500.0 °C | 37.8 W/(m·K) Show Material materials with Thermal conductivity of 37.8 W/(m·K) | ||
600.0 °C | 35.6 W/(m·K) Show Material materials with Thermal conductivity of 35.6 W/(m·K) | ||
Thermal diffusivity | 20.0 °C | 11.4 mm²/s Show Material materials with Thermal diffusivity of 11.4 mm²/s | |
100.0 °C | 11 mm²/s Show Material materials with Thermal diffusivity of 11 mm²/s | ||
200.0 °C | 10.3 mm²/s Show Material materials with Thermal diffusivity of 10.3 mm²/s | ||
300.0 °C | 9.5 mm²/s Show Material materials with Thermal diffusivity of 9.5 mm²/s | ||
400.0 °C | 8.5 mm²/s Show Material materials with Thermal diffusivity of 8.5 mm²/s | ||
500.0 °C | 7.3 mm²/s Show Material materials with Thermal diffusivity of 7.3 mm²/s | ||
600.0 °C | 6 mm²/s Show Material materials with Thermal diffusivity of 6 mm²/s | ||
Electrical
Property | Temperature | Value |
---|---|---|
Electrical resistivity | 20.0 °C | 2.54E-7 Ω·m Show Material materials with Electrical resistivity of 2.54E-7 Ω·m |
100.0 °C | 3E-7 Ω·m Show Material materials with Electrical resistivity of 3E-7 Ω·m | |
200.0 °C | 3.69E-7 Ω·m Show Material materials with Electrical resistivity of 3.69E-7 Ω·m | |
300.0 °C | 4.51E-7 Ω·m Show Material materials with Electrical resistivity of 4.51E-7 Ω·m | |
400.0 °C | 5.45E-7 Ω·m Show Material materials with Electrical resistivity of 5.45E-7 Ω·m | |
500.0 °C | 6.54E-7 Ω·m Show Material materials with Electrical resistivity of 6.54E-7 Ω·m | |
600.0 °C | 7.78E-7 Ω·m Show Material materials with Electrical resistivity of 7.78E-7 Ω·m | |
Chemical properties
Property | Value |
---|---|
Carbon | 0.17 - 0.22 % Show Material materials with Carbon of 0.17 - 0.22 % |
Chromium | 0.3 - 0.6 % Show Material materials with Chromium of 0.3 - 0.6 % |
Manganese | 0.7 - 1 % Show Material materials with Manganese of 0.7 - 1 % |
Molybdenum | 0.4 - 0.5 % Show Material materials with Molybdenum of 0.4 - 0.5 % |
Phosphorus | 0.04 % Show Material materials with Phosphorus of 0.04 % |
Silicon | 0.4 % Show Material materials with Silicon of 0.4 % |
Sulfur | 0.02 - 0.035 % Show Material materials with Sulfur of 0.02 - 0.035 % |