General
Property | Temperature | Value |
---|---|---|
Density | 20.0 °C | 7.84 g/cm³ Show Material materials with Density of 7.84 g/cm³ |
Mechanical
Property | Temperature | Value |
---|---|---|
Elastic modulus | -100.0 °C | 217 GPa Show Material materials with Elastic modulus of 217 GPa |
20.0 °C | 212 - 212.78 GPa Show Material materials with Elastic modulus of 212 - 212.78 GPa | |
100.0 °C | 207 GPa Show Material materials with Elastic modulus of 207 GPa | |
200.0 °C | 199 GPa Show Material materials with Elastic modulus of 199 GPa | |
300.0 °C | 192 GPa Show Material materials with Elastic modulus of 192 GPa | |
400.0 °C | 184 GPa Show Material materials with Elastic modulus of 184 GPa | |
500.0 °C | 175 GPa Show Material materials with Elastic modulus of 175 GPa | |
600.0 °C | 164 GPa Show Material materials with Elastic modulus of 164 GPa | |
Hardness, Brinell | 20.0 °C | 145 - 292 [-] Show Material materials with Hardness, Brinell of 145 - 292 [-] |
Poisson's ratio | 20.0 °C | 0.29 [-] Show Material materials with Poisson's ratio of 0.29 [-] |
Shear modulus | 20.0 °C | 82.8 GPa Show Material materials with Shear modulus of 82.8 GPa |
Thermal
Property | Temperature | Value | Comment |
---|---|---|---|
Coefficient of thermal expansion | -100.0 °C | 1.05E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.05E-5 1/K | |
20.0 °C | 1.15E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.15E-5 1/K | ||
100.0 °C | 1.21E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.21E-5 1/K | ||
200.0 °C | 1.27E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.27E-5 1/K | ||
300.0 °C | 1.32E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.32E-5 1/K | ||
400.0 °C | 1.36E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.36E-5 1/K | ||
500.0 °C | 1.4E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.4E-5 1/K | ||
600.0 °C | 1.44E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.44E-5 1/K | ||
Max service temperature, long | -60 - 0 °C Show Material materials with Max service temperature, long of -60 - 0 °C | ||
Melting point | 1382 - 1529 °C Show Material materials with Melting point of 1382 - 1529 °C | Typical for Nickel Chromium Molybdenum Steel | |
Specific heat capacity | -100.0 °C | 423 J/(kg·K) Show Material materials with Specific heat capacity of 423 J/(kg·K) | |
20.0 °C | 461 J/(kg·K) Show Material materials with Specific heat capacity of 461 J/(kg·K) | ||
100.0 °C | 479 J/(kg·K) Show Material materials with Specific heat capacity of 479 J/(kg·K) | ||
200.0 °C | 499 J/(kg·K) Show Material materials with Specific heat capacity of 499 J/(kg·K) | ||
300.0 °C | 517 J/(kg·K) Show Material materials with Specific heat capacity of 517 J/(kg·K) | ||
400.0 °C | 536 J/(kg·K) Show Material materials with Specific heat capacity of 536 J/(kg·K) | ||
500.0 °C | 558 J/(kg·K) Show Material materials with Specific heat capacity of 558 J/(kg·K) | ||
600.0 °C | 587 J/(kg·K) Show Material materials with Specific heat capacity of 587 J/(kg·K) | ||
Thermal conductivity | 20.0 °C | 46.3 W/(m·K) Show Material materials with Thermal conductivity of 46.3 W/(m·K) | |
100.0 °C | 47.1 W/(m·K) Show Material materials with Thermal conductivity of 47.1 W/(m·K) | ||
200.0 °C | 46.2 W/(m·K) Show Material materials with Thermal conductivity of 46.2 W/(m·K) | ||
300.0 °C | 44.1 W/(m·K) Show Material materials with Thermal conductivity of 44.1 W/(m·K) | ||
400.0 °C | 41.3 W/(m·K) Show Material materials with Thermal conductivity of 41.3 W/(m·K) | ||
500.0 °C | 38.6 W/(m·K) Show Material materials with Thermal conductivity of 38.6 W/(m·K) | ||
600.0 °C | 35.9 W/(m·K) Show Material materials with Thermal conductivity of 35.9 W/(m·K) | ||
Thermal diffusivity | 20.0 °C | 12.8 mm²/s Show Material materials with Thermal diffusivity of 12.8 mm²/s | |
100.0 °C | 12.1 mm²/s Show Material materials with Thermal diffusivity of 12.1 mm²/s | ||
200.0 °C | 11.1 mm²/s Show Material materials with Thermal diffusivity of 11.1 mm²/s | ||
300.0 °C | 10 mm²/s Show Material materials with Thermal diffusivity of 10 mm²/s | ||
400.0 °C | 8.8 mm²/s Show Material materials with Thermal diffusivity of 8.8 mm²/s | ||
500.0 °C | 7.4 mm²/s Show Material materials with Thermal diffusivity of 7.4 mm²/s | ||
600.0 °C | 4.7 mm²/s Show Material materials with Thermal diffusivity of 4.7 mm²/s | ||
Electrical
Property | Temperature | Value |
---|---|---|
Electrical resistivity | 20.0 °C | 2.25E-7 Ω·m Show Material materials with Electrical resistivity of 2.25E-7 Ω·m |
100.0 °C | 2.72E-7 Ω·m Show Material materials with Electrical resistivity of 2.72E-7 Ω·m | |
200.0 °C | 3.42E-7 Ω·m Show Material materials with Electrical resistivity of 3.42E-7 Ω·m | |
300.0 °C | 4.26E-7 Ω·m Show Material materials with Electrical resistivity of 4.26E-7 Ω·m | |
400.0 °C | 5.26E-7 Ω·m Show Material materials with Electrical resistivity of 5.26E-7 Ω·m | |
500.0 °C | 6.4E-7 Ω·m Show Material materials with Electrical resistivity of 6.4E-7 Ω·m | |
600.0 °C | 7.73E-7 Ω·m Show Material materials with Electrical resistivity of 7.73E-7 Ω·m | |
Chemical properties
Property | Value |
---|---|
Carbon | 0.17 - 0.23 % Show Material materials with Carbon of 0.17 - 0.23 % |
Chromium | 0.4 - 0.7 % Show Material materials with Chromium of 0.4 - 0.7 % |
Manganese | 0.65 - 0.95 % Show Material materials with Manganese of 0.65 - 0.95 % |
Molybdenum | 0.15 - 0.25 % Show Material materials with Molybdenum of 0.15 - 0.25 % |
Nickel | 0.4 - 0.7 % Show Material materials with Nickel of 0.4 - 0.7 % |
Phosphorus | 0.04 % Show Material materials with Phosphorus of 0.04 % |
Silicon | 0.4 % Show Material materials with Silicon of 0.4 % |
Sulfur | 0.035 % Show Material materials with Sulfur of 0.035 % |
Do you have a technical question or need more information about this material?
Post it as a comment below and receive answers from engineers and other community members.