General
Property | Temperature | Value |
---|---|---|
Density | 20.0 °C | 7.93 g/cm³ Show Material materials with Density of 7.93 g/cm³ |
Mechanical
Property | Temperature | Value |
---|---|---|
Elastic modulus | -100.0 °C | 206 GPa Show Material materials with Elastic modulus of 206 GPa |
20.0 °C | 196 - 202.24 GPa Show Material materials with Elastic modulus of 196 - 202.24 GPa | |
100.0 °C | 190 - 194.36 GPa Show Material materials with Elastic modulus of 190 - 194.36 GPa | |
200.0 °C | 182 - 186 GPa Show Material materials with Elastic modulus of 182 - 186 GPa | |
300.0 °C | 174 - 179 GPa Show Material materials with Elastic modulus of 174 - 179 GPa | |
400.0 °C | 166 - 172 GPa Show Material materials with Elastic modulus of 166 - 172 GPa | |
500.0 °C | 157.59 - 165 GPa Show Material materials with Elastic modulus of 157.59 - 165 GPa | |
600.0 °C | 149.24 - 150 GPa Show Material materials with Elastic modulus of 149.24 - 150 GPa | |
700.0 °C | 142 GPa Show Material materials with Elastic modulus of 142 GPa | |
800.0 °C | 134 GPa Show Material materials with Elastic modulus of 134 GPa | |
900.0 °C | 127 GPa Show Material materials with Elastic modulus of 127 GPa | |
1000.0 °C | 120 GPa Show Material materials with Elastic modulus of 120 GPa | |
Poisson's ratio | 20.0 °C | 0.29 [-] Show Material materials with Poisson's ratio of 0.29 [-] |
100.0 °C | 0.29 [-] Show Material materials with Poisson's ratio of 0.29 [-] | |
200.0 °C | 0.3 [-] Show Material materials with Poisson's ratio of 0.3 [-] | |
300.0 °C | 0.3 [-] Show Material materials with Poisson's ratio of 0.3 [-] | |
400.0 °C | 0.31 [-] Show Material materials with Poisson's ratio of 0.31 [-] | |
500.0 °C | 0.32 [-] Show Material materials with Poisson's ratio of 0.32 [-] | |
600.0 °C | 0.33 [-] Show Material materials with Poisson's ratio of 0.33 [-] | |
Reduction of area | 20.0 °C | 55 % Show Material materials with Reduction of area of 55 % |
Shear modulus | 20.0 °C | 78.33 GPa Show Material materials with Shear modulus of 78.33 GPa |
100.0 °C | 75.08 GPa Show Material materials with Shear modulus of 75.08 GPa | |
200.0 °C | 71.07 GPa Show Material materials with Shear modulus of 71.07 GPa | |
300.0 °C | 67.21 GPa Show Material materials with Shear modulus of 67.21 GPa | |
400.0 °C | 63.34 GPa Show Material materials with Shear modulus of 63.34 GPa | |
500.0 °C | 59.64 GPa Show Material materials with Shear modulus of 59.64 GPa | |
600.0 °C | 56.08 GPa Show Material materials with Shear modulus of 56.08 GPa | |
Tensile strength | 20.0 °C | 650 MPa Show Material materials with Tensile strength of 650 MPa |
Thermal
Property | Temperature | Value | Comment |
---|---|---|---|
Coefficient of thermal expansion | -100.0 °C | 1.49E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.49E-5 1/K | |
20.0 °C | 1.61E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.61E-5 1/K | ||
100.0 °C | 1.6E-5 - 1.67E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.6E-5 - 1.67E-5 1/K | ||
200.0 °C | 1.7E-5 - 1.72E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.7E-5 - 1.72E-5 1/K | ||
300.0 °C | 1.7E-5 - 1.77E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.7E-5 - 1.77E-5 1/K | ||
400.0 °C | 1.8E-5 - 1.81E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.8E-5 - 1.81E-5 1/K | ||
500.0 °C | 1.8E-5 - 1.84E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.8E-5 - 1.84E-5 1/K | ||
600.0 °C | 1.88E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.88E-5 1/K | ||
700.0 °C | 1.91E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.91E-5 1/K | ||
800.0 °C | 1.94E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.94E-5 1/K | ||
900.0 °C | 1.97E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.97E-5 1/K | ||
1000.0 °C | 2E-5 1/K Show Material materials with Coefficient of thermal expansion of 2E-5 1/K | ||
Melting point | 1230 - 1480 °C Show Material materials with Melting point of 1230 - 1480 °C | Typical for Austenitic Stainless Steel | |
Specific heat capacity | -100.0 °C | 440 J/(kg·K) Show Material materials with Specific heat capacity of 440 J/(kg·K) | |
20.0 °C | 472 J/(kg·K) Show Material materials with Specific heat capacity of 472 J/(kg·K) | ||
100.0 °C | 487 J/(kg·K) Show Material materials with Specific heat capacity of 487 J/(kg·K) | ||
200.0 °C | 503 J/(kg·K) Show Material materials with Specific heat capacity of 503 J/(kg·K) | ||
300.0 °C | 512 J/(kg·K) Show Material materials with Specific heat capacity of 512 J/(kg·K) | ||
400.0 °C | 520 J/(kg·K) Show Material materials with Specific heat capacity of 520 J/(kg·K) | ||
500.0 °C | 530 J/(kg·K) Show Material materials with Specific heat capacity of 530 J/(kg·K) | ||
600.0 °C | 541 J/(kg·K) Show Material materials with Specific heat capacity of 541 J/(kg·K) | ||
700.0 °C | 551 J/(kg·K) Show Material materials with Specific heat capacity of 551 J/(kg·K) | ||
800.0 °C | 559 J/(kg·K) Show Material materials with Specific heat capacity of 559 J/(kg·K) | ||
900.0 °C | 565 J/(kg·K) Show Material materials with Specific heat capacity of 565 J/(kg·K) | ||
1000.0 °C | 571 J/(kg·K) Show Material materials with Specific heat capacity of 571 J/(kg·K) | ||
Thermal conductivity | 20.0 °C | 14.3 W/(m·K) Show Material materials with Thermal conductivity of 14.3 W/(m·K) | |
100.0 °C | 15.8 W/(m·K) Show Material materials with Thermal conductivity of 15.8 W/(m·K) | ||
200.0 °C | 17.5 W/(m·K) Show Material materials with Thermal conductivity of 17.5 W/(m·K) | ||
300.0 °C | 19 W/(m·K) Show Material materials with Thermal conductivity of 19 W/(m·K) | ||
400.0 °C | 20.5 W/(m·K) Show Material materials with Thermal conductivity of 20.5 W/(m·K) | ||
500.0 °C | 21.9 W/(m·K) Show Material materials with Thermal conductivity of 21.9 W/(m·K) | ||
600.0 °C | 23.3 W/(m·K) Show Material materials with Thermal conductivity of 23.3 W/(m·K) | ||
700.0 °C | 24.6 W/(m·K) Show Material materials with Thermal conductivity of 24.6 W/(m·K) | ||
800.0 °C | 26 W/(m·K) Show Material materials with Thermal conductivity of 26 W/(m·K) | ||
900.0 °C | 27.4 W/(m·K) Show Material materials with Thermal conductivity of 27.4 W/(m·K) | ||
1000.0 °C | 28.8 W/(m·K) Show Material materials with Thermal conductivity of 28.8 W/(m·K) | ||
Thermal diffusivity | 20.0 °C | 3.8 mm²/s Show Material materials with Thermal diffusivity of 3.8 mm²/s | |
100.0 °C | 4 mm²/s Show Material materials with Thermal diffusivity of 4 mm²/s | ||
200.0 °C | 4.2 mm²/s Show Material materials with Thermal diffusivity of 4.2 mm²/s | ||
300.0 °C | 4.6 mm²/s Show Material materials with Thermal diffusivity of 4.6 mm²/s | ||
400.0 °C | 4.8 mm²/s Show Material materials with Thermal diffusivity of 4.8 mm²/s | ||
500.0 °C | 4.9 mm²/s Show Material materials with Thermal diffusivity of 4.9 mm²/s | ||
600.0 °C | 5 mm²/s Show Material materials with Thermal diffusivity of 5 mm²/s | ||
700.0 °C | 5.3 mm²/s Show Material materials with Thermal diffusivity of 5.3 mm²/s | ||
800.0 °C | 5.6 mm²/s Show Material materials with Thermal diffusivity of 5.6 mm²/s | ||
900.0 °C | 5.9 mm²/s Show Material materials with Thermal diffusivity of 5.9 mm²/s | ||
1000.0 °C | 6 mm²/s Show Material materials with Thermal diffusivity of 6 mm²/s | ||
Electrical
Property | Temperature | Value |
---|---|---|
Electrical resistivity | 20.0 °C | 7.1E-7 Ω·m Show Material materials with Electrical resistivity of 7.1E-7 Ω·m |
100.0 °C | 7.76E-7 Ω·m Show Material materials with Electrical resistivity of 7.76E-7 Ω·m | |
200.0 °C | 8.49E-7 Ω·m Show Material materials with Electrical resistivity of 8.49E-7 Ω·m | |
300.0 °C | 9.14E-7 Ω·m Show Material materials with Electrical resistivity of 9.14E-7 Ω·m | |
400.0 °C | 9.71E-7 Ω·m Show Material materials with Electrical resistivity of 9.71E-7 Ω·m | |
500.0 °C | 1.02E-6 Ω·m Show Material materials with Electrical resistivity of 1.02E-6 Ω·m | |
600.0 °C | 1.07E-6 Ω·m Show Material materials with Electrical resistivity of 1.07E-6 Ω·m | |
700.0 °C | 1.1E-6 Ω·m Show Material materials with Electrical resistivity of 1.1E-6 Ω·m | |
800.0 °C | 1.14E-6 Ω·m Show Material materials with Electrical resistivity of 1.14E-6 Ω·m | |
900.0 °C | 1.17E-6 Ω·m Show Material materials with Electrical resistivity of 1.17E-6 Ω·m | |
1000.0 °C | 1.19E-6 Ω·m Show Material materials with Electrical resistivity of 1.19E-6 Ω·m | |
Chemical properties
Property | Value |
---|---|
Carbon | 0.07 % Show Material materials with Carbon of 0.07 % |
Chromium | 17 - 19 % Show Material materials with Chromium of 17 - 19 % |
Manganese | 2 % Show Material materials with Manganese of 2 % |
Nickel | 11 - 13 % Show Material materials with Nickel of 11 - 13 % |
Phosphorus | 0.05 % Show Material materials with Phosphorus of 0.05 % |
Silicon | 1 % Show Material materials with Silicon of 1 % |
Sulfur | 0.03 % Show Material materials with Sulfur of 0.03 % |
Do you have a technical question or need more information about this material?
Post it as a comment below and receive answers from engineers and other community members.