General
Property | Temperature | Value |
---|---|---|
Density | 20.0 °C | 7.84 g/cm³ Show Material materials with Density of 7.84 g/cm³ |
Mechanical
Property | Temperature | Value | Comment |
---|---|---|---|
Elastic modulus | -100.0 °C | 217 GPa Show Material materials with Elastic modulus of 217 GPa | |
20.0 °C | 212 GPa Show Material materials with Elastic modulus of 212 GPa | ||
100.0 °C | 207 GPa Show Material materials with Elastic modulus of 207 GPa | ||
200.0 °C | 199 GPa Show Material materials with Elastic modulus of 199 GPa | ||
300.0 °C | 192 GPa Show Material materials with Elastic modulus of 192 GPa | ||
400.0 °C | 184 GPa Show Material materials with Elastic modulus of 184 GPa | ||
500.0 °C | 175 GPa Show Material materials with Elastic modulus of 175 GPa | ||
600.0 °C | 164 GPa Show Material materials with Elastic modulus of 164 GPa | ||
Elongation | 20.0 °C | 16 % Show Material materials with Elongation of 16 % | |
Poisson's ratio | 23.0 °C | 0.3 [-] Show Material materials with Poisson's ratio of 0.3 [-] | Typical for Steel |
Tensile strength | 20.0 °C | 570 - 780 MPa Show Material materials with Tensile strength of 570 - 780 MPa | |
Yield strength | 20.0 °C | 410 - 500 MPa Show Material materials with Yield strength of 410 - 500 MPa | |
Yield strength Rp0.2 | 100.0 °C | 373 - 422 MPa Show Material materials with Yield strength Rp0.2 of 373 - 422 MPa | |
150.0 °C | 343 - 392 MPa Show Material materials with Yield strength Rp0.2 of 343 - 392 MPa | ||
200.0 °C | 324 - 363 MPa Show Material materials with Yield strength Rp0.2 of 324 - 363 MPa | ||
250.0 °C | 294 - 333 MPa Show Material materials with Yield strength Rp0.2 of 294 - 333 MPa | ||
300.0 °C | 275 - 314 MPa Show Material materials with Yield strength Rp0.2 of 275 - 314 MPa | ||
350.0 °C | 245 - 284 MPa Show Material materials with Yield strength Rp0.2 of 245 - 284 MPa | ||
400.0 °C | 206 - 255 MPa Show Material materials with Yield strength Rp0.2 of 206 - 255 MPa | ||
Thermal
Property | Temperature | Value |
---|---|---|
Coefficient of thermal expansion | -100.0 °C | 1.05E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.05E-5 1/K |
20.0 °C | 1.15E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.15E-5 1/K | |
100.0 °C | 1.21E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.21E-5 1/K | |
200.0 °C | 1.27E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.27E-5 1/K | |
300.0 °C | 1.32E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.32E-5 1/K | |
400.0 °C | 1.36E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.36E-5 1/K | |
500.0 °C | 1.4E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.4E-5 1/K | |
600.0 °C | 1.44E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.44E-5 1/K | |
Max service temperature, long | 0 - 400 °C Show Material materials with Max service temperature, long of 0 - 400 °C | |
Specific heat capacity | -100.0 °C | 423 J/(kg·K) Show Material materials with Specific heat capacity of 423 J/(kg·K) |
20.0 °C | 461 J/(kg·K) Show Material materials with Specific heat capacity of 461 J/(kg·K) | |
100.0 °C | 479 J/(kg·K) Show Material materials with Specific heat capacity of 479 J/(kg·K) | |
200.0 °C | 499 J/(kg·K) Show Material materials with Specific heat capacity of 499 J/(kg·K) | |
300.0 °C | 517 J/(kg·K) Show Material materials with Specific heat capacity of 517 J/(kg·K) | |
400.0 °C | 536 J/(kg·K) Show Material materials with Specific heat capacity of 536 J/(kg·K) | |
500.0 °C | 558 J/(kg·K) Show Material materials with Specific heat capacity of 558 J/(kg·K) | |
600.0 °C | 587 J/(kg·K) Show Material materials with Specific heat capacity of 587 J/(kg·K) | |
Thermal conductivity | -100.0 °C | 34.7 W/(m·K) Show Material materials with Thermal conductivity of 34.7 W/(m·K) |
20.0 °C | 39.7 W/(m·K) Show Material materials with Thermal conductivity of 39.7 W/(m·K) | |
100.0 °C | 40.9 W/(m·K) Show Material materials with Thermal conductivity of 40.9 W/(m·K) | |
200.0 °C | 41 W/(m·K) Show Material materials with Thermal conductivity of 41 W/(m·K) | |
300.0 °C | 39.9 W/(m·K) Show Material materials with Thermal conductivity of 39.9 W/(m·K) | |
400.0 °C | 38.2 W/(m·K) Show Material materials with Thermal conductivity of 38.2 W/(m·K) | |
500.0 °C | 36.1 W/(m·K) Show Material materials with Thermal conductivity of 36.1 W/(m·K) | |
600.0 °C | 33.8 W/(m·K) Show Material materials with Thermal conductivity of 33.8 W/(m·K) | |
Thermal diffusivity | -100.0 °C | 11.9 mm²/s Show Material materials with Thermal diffusivity of 11.9 mm²/s |
20.0 °C | 11 mm²/s Show Material materials with Thermal diffusivity of 11 mm²/s | |
100.0 °C | 10.5 mm²/s Show Material materials with Thermal diffusivity of 10.5 mm²/s | |
200.0 °C | 9.9 mm²/s Show Material materials with Thermal diffusivity of 9.9 mm²/s | |
300.0 °C | 9.1 mm²/s Show Material materials with Thermal diffusivity of 9.1 mm²/s | |
400.0 °C | 8.1 mm²/s Show Material materials with Thermal diffusivity of 8.1 mm²/s | |
500.0 °C | 6.9 mm²/s Show Material materials with Thermal diffusivity of 6.9 mm²/s | |
600.0 °C | 5.7 mm²/s Show Material materials with Thermal diffusivity of 5.7 mm²/s | |
Electrical
Property | Temperature | Value |
---|---|---|
Electrical resistivity | -100.0 °C | 1.97E-7 Ω·m Show Material materials with Electrical resistivity of 1.97E-7 Ω·m |
20.0 °C | 2.62E-7 Ω·m Show Material materials with Electrical resistivity of 2.62E-7 Ω·m | |
100.0 °C | 3.13E-7 Ω·m Show Material materials with Electrical resistivity of 3.13E-7 Ω·m | |
200.0 °C | 3.85E-7 Ω·m Show Material materials with Electrical resistivity of 3.85E-7 Ω·m | |
300.0 °C | 4.7E-7 Ω·m Show Material materials with Electrical resistivity of 4.7E-7 Ω·m | |
400.0 °C | 5.69E-7 Ω·m Show Material materials with Electrical resistivity of 5.69E-7 Ω·m | |
500.0 °C | 6.85E-7 Ω·m Show Material materials with Electrical resistivity of 6.85E-7 Ω·m | |
600.0 °C | 8.2E-7 Ω·m Show Material materials with Electrical resistivity of 8.2E-7 Ω·m | |
Chemical properties
Property | Value |
---|---|
Aluminium | 0.02 % Show Material materials with Aluminium of 0.02 % |
Carbon | 0.21 % Show Material materials with Carbon of 0.21 % |
Chromium | 0.3 % Show Material materials with Chromium of 0.3 % |
Copper | 0.2 % Show Material materials with Copper of 0.2 % |
Manganese | 1 - 1.7 % Show Material materials with Manganese of 1 - 1.7 % |
Molybdenum | 0.1 % Show Material materials with Molybdenum of 0.1 % |
Nickel | 1 % Show Material materials with Nickel of 1 % |
Niobium | 0.05 % Show Material materials with Niobium of 0.05 % |
Nitrogen | 0.02 % Show Material materials with Nitrogen of 0.02 % |
Phosphorus | 0.04 % Show Material materials with Phosphorus of 0.04 % |
Silicon | 0.1 - 0.6 % Show Material materials with Silicon of 0.1 - 0.6 % |
Sulfur | 0.03 % Show Material materials with Sulfur of 0.03 % |
Vanadium | 0.22 % Show Material materials with Vanadium of 0.22 % |
Do you have a technical question or need more information about this material?
Post it as a comment below and receive answers from engineers and other community members.