General
Property | Temperature | Value |
---|---|---|
Density | 20.0 °C | 7.85 g/cm³ Show Material materials with Density of 7.85 g/cm³ |
Mechanical
Property | Temperature | Value | Comment |
---|---|---|---|
Elastic modulus | -100.0 °C | 217 GPa Show Material materials with Elastic modulus of 217 GPa | |
20.0 °C | 212 GPa Show Material materials with Elastic modulus of 212 GPa | ||
100.0 °C | 207 GPa Show Material materials with Elastic modulus of 207 GPa | ||
200.0 °C | 199 - 200 GPa Show Material materials with Elastic modulus of 199 - 200 GPa | ||
300.0 °C | 192 GPa Show Material materials with Elastic modulus of 192 GPa | ||
400.0 °C | 183 - 184 GPa Show Material materials with Elastic modulus of 183 - 184 GPa | ||
500.0 °C | 175 GPa Show Material materials with Elastic modulus of 175 GPa | ||
600.0 °C | 164 - 166 GPa Show Material materials with Elastic modulus of 164 - 166 GPa | ||
Elongation | 20.0 °C | 25 % Show Material materials with Elongation of 25 % | |
Elongation, transverse | 20.0 °C | 23 % Show Material materials with Elongation, transverse of 23 % | |
Poisson's ratio | 20.0 °C | 0.28 [-] Show Material materials with Poisson's ratio of 0.28 [-] | |
Shear modulus | 23.0 °C | 82 GPa Show Material materials with Shear modulus of 82 GPa | Typical for Low Carbon Steel |
Tensile strength | 20.0 °C | 360 - 520 MPa Show Material materials with Tensile strength of 360 - 520 MPa | |
Yield strength | 20.0 °C | 235 MPa Show Material materials with Yield strength of 235 MPa | |
Yield strength Rp0.2 | 20.0 °C | 215 - 235 MPa Show Material materials with Yield strength Rp0.2 of 215 - 235 MPa | |
100.0 °C | 205 MPa Show Material materials with Yield strength Rp0.2 of 205 MPa | ||
200.0 °C | 175 - 185 MPa Show Material materials with Yield strength Rp0.2 of 175 - 185 MPa | ||
250.0 °C | 155 - 165 MPa Show Material materials with Yield strength Rp0.2 of 155 - 165 MPa | ||
300.0 °C | 130 - 140 MPa Show Material materials with Yield strength Rp0.2 of 130 - 140 MPa | ||
350.0 °C | 115 - 120 MPa Show Material materials with Yield strength Rp0.2 of 115 - 120 MPa | ||
400.0 °C | 110 MPa Show Material materials with Yield strength Rp0.2 of 110 MPa | ||
450.0 °C | 105 MPa Show Material materials with Yield strength Rp0.2 of 105 MPa | ||
Thermal
Property | Temperature | Value | Comment |
---|---|---|---|
Coefficient of thermal expansion | -100.0 °C | 1.08E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.08E-5 1/K | |
20.0 °C | 1.19E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.19E-5 1/K | ||
100.0 °C | 1.22E-5 - 1.25E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.22E-5 - 1.25E-5 1/K | ||
200.0 °C | 1.29E-5 - 1.3E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.29E-5 - 1.3E-5 1/K | ||
300.0 °C | 1.34E-5 - 1.36E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.34E-5 - 1.36E-5 1/K | ||
400.0 °C | 1.4E-5 - 1.41E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.4E-5 - 1.41E-5 1/K | ||
500.0 °C | 1.43E-5 - 1.45E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.43E-5 - 1.45E-5 1/K | ||
600.0 °C | 1.46E-5 - 1.49E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.46E-5 - 1.49E-5 1/K | ||
Max service temperature | 500 °C Show Material materials with Max service temperature of 500 °C | Typical for Carbon Steel | |
Max service temperature, long | 0 - 500 °C Show Material materials with Max service temperature, long of 0 - 500 °C | ||
Melting point | 1480 - 1526 °C Show Material materials with Melting point of 1480 - 1526 °C | Typical for Low Carbon Steel | |
Specific heat capacity | -100.0 °C | 423 J/(kg·K) Show Material materials with Specific heat capacity of 423 J/(kg·K) | |
20.0 °C | 461 J/(kg·K) Show Material materials with Specific heat capacity of 461 J/(kg·K) | ||
100.0 °C | 479 - 500 J/(kg·K) Show Material materials with Specific heat capacity of 479 - 500 J/(kg·K) | ||
200.0 °C | 499 - 540 J/(kg·K) Show Material materials with Specific heat capacity of 499 - 540 J/(kg·K) | ||
300.0 °C | 517 - 580 J/(kg·K) Show Material materials with Specific heat capacity of 517 - 580 J/(kg·K) | ||
400.0 °C | 536 - 620 J/(kg·K) Show Material materials with Specific heat capacity of 536 - 620 J/(kg·K) | ||
500.0 °C | 558 - 690 J/(kg·K) Show Material materials with Specific heat capacity of 558 - 690 J/(kg·K) | ||
600.0 °C | 587 - 780 J/(kg·K) Show Material materials with Specific heat capacity of 587 - 780 J/(kg·K) | ||
Thermal conductivity | 20.0 °C | 56.9 W/(m·K) Show Material materials with Thermal conductivity of 56.9 W/(m·K) | |
100.0 °C | 56.4 - 57 W/(m·K) Show Material materials with Thermal conductivity of 56.4 - 57 W/(m·K) | ||
200.0 °C | 53.5 - 54 W/(m·K) Show Material materials with Thermal conductivity of 53.5 - 54 W/(m·K) | ||
300.0 °C | 49.4 - 50 W/(m·K) Show Material materials with Thermal conductivity of 49.4 - 50 W/(m·K) | ||
400.0 °C | 45 - 45.2 W/(m·K) Show Material materials with Thermal conductivity of 45 - 45.2 W/(m·K) | ||
500.0 °C | 41.3 - 42 W/(m·K) Show Material materials with Thermal conductivity of 41.3 - 42 W/(m·K) | ||
600.0 °C | 37 - 37.6 W/(m·K) Show Material materials with Thermal conductivity of 37 - 37.6 W/(m·K) | ||
Thermal diffusivity | 20.0 °C | 15.7 mm²/s Show Material materials with Thermal diffusivity of 15.7 mm²/s | |
100.0 °C | 14.5 mm²/s Show Material materials with Thermal diffusivity of 14.5 mm²/s | ||
200.0 °C | 12.9 mm²/s Show Material materials with Thermal diffusivity of 12.9 mm²/s | ||
300.0 °C | 11.2 mm²/s Show Material materials with Thermal diffusivity of 11.2 mm²/s | ||
400.0 °C | 9.6 mm²/s Show Material materials with Thermal diffusivity of 9.6 mm²/s | ||
500.0 °C | 7.9 mm²/s Show Material materials with Thermal diffusivity of 7.9 mm²/s | ||
600.0 °C | 6.3 mm²/s Show Material materials with Thermal diffusivity of 6.3 mm²/s | ||
Electrical
Property | Temperature | Value |
---|---|---|
Electrical resistivity | 20.0 °C | 1.83E-7 Ω·m Show Material materials with Electrical resistivity of 1.83E-7 Ω·m |
100.0 °C | 2.27E-7 - 2.3E-7 Ω·m Show Material materials with Electrical resistivity of 2.27E-7 - 2.3E-7 Ω·m | |
200.0 °C | 2.95E-7 - 3E-7 Ω·m Show Material materials with Electrical resistivity of 2.95E-7 - 3E-7 Ω·m | |
300.0 °C | 3.8E-7 Ω·m Show Material materials with Electrical resistivity of 3.8E-7 Ω·m | |
400.0 °C | 4.8E-7 - 4.81E-7 Ω·m Show Material materials with Electrical resistivity of 4.8E-7 - 4.81E-7 Ω·m | |
500.0 °C | 5.99E-7 - 6E-7 Ω·m Show Material materials with Electrical resistivity of 5.99E-7 - 6E-7 Ω·m | |
600.0 °C | 7.38E-7 - 7.4E-7 Ω·m Show Material materials with Electrical resistivity of 7.38E-7 - 7.4E-7 Ω·m | |
Magnetic
Property | Value | Comment |
---|---|---|
Curie temperature | 770 °C Show Material materials with Curie temperature of 770 °C | Typical for Low Carbon Steel |
Chemical properties
Property | Value |
---|---|
Aluminium | 0.02 % Show Material materials with Aluminium of 0.02 % |
Carbon | 0.17 % Show Material materials with Carbon of 0.17 % |
Manganese | 0.4 - 0.8 % Show Material materials with Manganese of 0.4 - 0.8 % |
Phosphorus | 0.04 % Show Material materials with Phosphorus of 0.04 % |
Silicon | 0.1 - 0.35 % Show Material materials with Silicon of 0.1 - 0.35 % |
Sulfur | 0.04 % Show Material materials with Sulfur of 0.04 % |