DIN 17176 Grade 12CrMo19-5 quenched and tempered (+QT1)

Want to keep this datasheet? Save it now in your required format

Description

High temperature steel for high pressure hydrogenation vessels. It is scale resistant up to 650 °C as well as chemical resistant to aggressive (e.g. sulphurous) oils. Application: hydration facilities and petroleum distillation facilities for tubes and shapes, in the quenched and tempered condition also in the steam boiler construction for overheater tubes and collectors

Related Standards

Equivalent Materials

This material data has been provided by WIAM.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValue

Density

20.0 °C

7.77 g/cm³

Show Material materials with Density of 7.77 g/cm³

Mechanical

PropertyTemperatureValue

Elastic modulus

20.0 °C

212 - 212.36 GPa

Show Material materials with Elastic modulus of 212 - 212.36 GPa

95.0 °C

208.22 GPa

Show Material materials with Elastic modulus of 208.22 GPa

100.0 °C

207 - 212 GPa

Show Material materials with Elastic modulus of 207 - 212 GPa

150.0 °C

204.77 GPa

Show Material materials with Elastic modulus of 204.77 GPa

200.0 °C

199 - 205 GPa

Show Material materials with Elastic modulus of 199 - 205 GPa

205.0 °C

200.64 GPa

Show Material materials with Elastic modulus of 200.64 GPa

260.0 °C

195.81 GPa

Show Material materials with Elastic modulus of 195.81 GPa

300.0 °C

192 - 198 GPa

Show Material materials with Elastic modulus of 192 - 198 GPa

315.0 °C

191.67 GPa

Show Material materials with Elastic modulus of 191.67 GPa

370.0 °C

187.54 GPa

Show Material materials with Elastic modulus of 187.54 GPa

400.0 °C

184 - 189 GPa

Show Material materials with Elastic modulus of 184 - 189 GPa

425.0 °C

182.71 GPa

Show Material materials with Elastic modulus of 182.71 GPa

485.0 °C

177.89 GPa

Show Material materials with Elastic modulus of 177.89 GPa

500.0 °C

175 - 180 GPa

Show Material materials with Elastic modulus of 175 - 180 GPa

540.0 °C

172.37 GPa

Show Material materials with Elastic modulus of 172.37 GPa

595.0 °C

166.85 GPa

Show Material materials with Elastic modulus of 166.85 GPa

600.0 °C

164 - 168 GPa

Show Material materials with Elastic modulus of 164 - 168 GPa

650.0 °C

159.96 GPa

Show Material materials with Elastic modulus of 159.96 GPa

705.0 °C

151.69 GPa

Show Material materials with Elastic modulus of 151.69 GPa

760.0 °C

139.27 GPa

Show Material materials with Elastic modulus of 139.27 GPa

Elongation

20.0 °C

17 - 20 %

Show Material materials with Elongation of 17 - 20 %

Elongation, transverse

20.0 °C

17 %

Show Material materials with Elongation, transverse of 17 %

Hardness, Brinell

20.0 °C

175 - 220 [-]

Show Material materials with Hardness, Brinell of 175 - 220 [-]

Poisson's ratio

20.0 °C

0.31 [-]

Show Material materials with Poisson's ratio of 0.31 [-]

95.0 °C

0.3 [-]

Show Material materials with Poisson's ratio of 0.3 [-]

150.0 °C

0.3 [-]

Show Material materials with Poisson's ratio of 0.3 [-]

205.0 °C

0.3 [-]

Show Material materials with Poisson's ratio of 0.3 [-]

260.0 °C

0.3 [-]

Show Material materials with Poisson's ratio of 0.3 [-]

315.0 °C

0.3 [-]

Show Material materials with Poisson's ratio of 0.3 [-]

370.0 °C

0.3 [-]

Show Material materials with Poisson's ratio of 0.3 [-]

425.0 °C

0.3 [-]

Show Material materials with Poisson's ratio of 0.3 [-]

485.0 °C

0.32 [-]

Show Material materials with Poisson's ratio of 0.32 [-]

540.0 °C

0.3 [-]

Show Material materials with Poisson's ratio of 0.3 [-]

595.0 °C

0.31 [-]

Show Material materials with Poisson's ratio of 0.31 [-]

650.0 °C

0.32 [-]

Show Material materials with Poisson's ratio of 0.32 [-]

705.0 °C

0.33 [-]

Show Material materials with Poisson's ratio of 0.33 [-]

760.0 °C

0.33 [-]

Show Material materials with Poisson's ratio of 0.33 [-]

Unlock all property charts

Shear modulus

20.0 °C

81.36 GPa

Show Material materials with Shear modulus of 81.36 GPa

95.0 °C

80.32 GPa

Show Material materials with Shear modulus of 80.32 GPa

150.0 °C

78.95 GPa

Show Material materials with Shear modulus of 78.95 GPa

205.0 °C

77.22 GPa

Show Material materials with Shear modulus of 77.22 GPa

260.0 °C

75.5 GPa

Show Material materials with Shear modulus of 75.5 GPa

315.0 °C

73.77 GPa

Show Material materials with Shear modulus of 73.77 GPa

370.0 °C

72.05 GPa

Show Material materials with Shear modulus of 72.05 GPa

425.0 °C

70.33 GPa

Show Material materials with Shear modulus of 70.33 GPa

485.0 °C

67.57 GPa

Show Material materials with Shear modulus of 67.57 GPa

540.0 °C

66.19 GPa

Show Material materials with Shear modulus of 66.19 GPa

595.0 °C

63.78 GPa

Show Material materials with Shear modulus of 63.78 GPa

650.0 °C

60.67 GPa

Show Material materials with Shear modulus of 60.67 GPa

705.0 °C

57.23 GPa

Show Material materials with Shear modulus of 57.23 GPa

760.0 °C

52.4 GPa

Show Material materials with Shear modulus of 52.4 GPa

Unlock all property charts

Tensile strength

20.0 °C

470 - 640 MPa

Show Material materials with Tensile strength of 470 - 640 MPa

100.0 °C

450 MPa

Show Material materials with Tensile strength of 450 MPa

150.0 °C

425 MPa

Show Material materials with Tensile strength of 425 MPa

200.0 °C

400 MPa

Show Material materials with Tensile strength of 400 MPa

250.0 °C

390 - 400 MPa

Show Material materials with Tensile strength of 390 - 400 MPa

300.0 °C

380 - 390 MPa

Show Material materials with Tensile strength of 380 - 390 MPa

350.0 °C

365 - 380 MPa

Show Material materials with Tensile strength of 365 - 380 MPa

400.0 °C

345 - 360 MPa

Show Material materials with Tensile strength of 345 - 360 MPa

450.0 °C

325 - 335 MPa

Show Material materials with Tensile strength of 325 - 335 MPa

500.0 °C

305 - 310 MPa

Show Material materials with Tensile strength of 305 - 310 MPa

Unlock all property charts

Tensile strength, transverse

20.0 °C

470 - 640 MPa

Show Material materials with Tensile strength, transverse of 470 - 640 MPa

Yield strength

20.0 °C

275 MPa

Show Material materials with Yield strength of 275 MPa

Yield strength Rp0.2

20.0 °C

275 MPa

Show Material materials with Yield strength Rp0.2 of 275 MPa

100.0 °C

245 MPa

Show Material materials with Yield strength Rp0.2 of 245 MPa

150.0 °C

237 MPa

Show Material materials with Yield strength Rp0.2 of 237 MPa

200.0 °C

230 MPa

Show Material materials with Yield strength Rp0.2 of 230 MPa

250.0 °C

223 MPa

Show Material materials with Yield strength Rp0.2 of 223 MPa

300.0 °C

216 MPa

Show Material materials with Yield strength Rp0.2 of 216 MPa

350.0 °C

206 MPa

Show Material materials with Yield strength Rp0.2 of 206 MPa

400.0 °C

196 MPa

Show Material materials with Yield strength Rp0.2 of 196 MPa

450.0 °C

181 MPa

Show Material materials with Yield strength Rp0.2 of 181 MPa

500.0 °C

167 MPa

Show Material materials with Yield strength Rp0.2 of 167 MPa

Unlock all property charts

Yield strength Rp0.2, transverse

20.0 °C

275 MPa

Show Material materials with Yield strength Rp0.2, transverse of 275 MPa

Thermal

PropertyTemperatureValueComment

Coefficient of thermal expansion

-100.0 °C

1E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1E-5 1/K

20.0 °C

1.08E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.08E-5 1/K

100.0 °C

1.13E-5 - 1.14E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.13E-5 - 1.14E-5 1/K

200.0 °C

1.18E-5 - 1.2E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.18E-5 - 1.2E-5 1/K

300.0 °C

1.23E-5 - 1.24E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.23E-5 - 1.24E-5 1/K

400.0 °C

1.27E-5 - 1.28E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.27E-5 - 1.28E-5 1/K

425.0 °C

1.24E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.24E-5 1/K

485.0 °C

1.26E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.26E-5 1/K

500.0 °C

1.3E-5 - 1.32E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.3E-5 - 1.32E-5 1/K

540.0 °C

1.28E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.28E-5 1/K

595.0 °C

1.29E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.29E-5 1/K

600.0 °C

1.32E-5 - 1.34E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.32E-5 - 1.34E-5 1/K

650.0 °C

1.32E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.32E-5 1/K

700.0 °C

1.33E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.33E-5 1/K

705.0 °C

1.32E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.32E-5 1/K

Unlock all property charts

Max service temperature, long

0 - 650 °C

Show Material materials with Max service temperature, long of 0 - 650 °C

Melting point

1382 - 1529 °C

Show Material materials with Melting point of 1382 - 1529 °C

Typical for Chromium Molybdenum Steel

Specific heat capacity

-100.0 °C

423 J/(kg·K)

Show Material materials with Specific heat capacity of 423 J/(kg·K)

20.0 °C

461 J/(kg·K)

Show Material materials with Specific heat capacity of 461 J/(kg·K)

100.0 °C

479 - 490 J/(kg·K)

Show Material materials with Specific heat capacity of 479 - 490 J/(kg·K)

200.0 °C

499 - 530 J/(kg·K)

Show Material materials with Specific heat capacity of 499 - 530 J/(kg·K)

300.0 °C

517 - 560 J/(kg·K)

Show Material materials with Specific heat capacity of 517 - 560 J/(kg·K)

400.0 °C

536 - 610 J/(kg·K)

Show Material materials with Specific heat capacity of 536 - 610 J/(kg·K)

500.0 °C

558 - 670 J/(kg·K)

Show Material materials with Specific heat capacity of 558 - 670 J/(kg·K)

600.0 °C

587 - 760 J/(kg·K)

Show Material materials with Specific heat capacity of 587 - 760 J/(kg·K)

Unlock all property charts

Thermal conductivity

20.0 °C

20.3 W/(m·K)

Show Material materials with Thermal conductivity of 20.3 W/(m·K)

100.0 °C

22.7 - 23 W/(m·K)

Show Material materials with Thermal conductivity of 22.7 - 23 W/(m·K)

200.0 °C

25 W/(m·K)

Show Material materials with Thermal conductivity of 25 W/(m·K)

300.0 °C

26 - 26.4 W/(m·K)

Show Material materials with Thermal conductivity of 26 - 26.4 W/(m·K)

400.0 °C

27 - 27.3 W/(m·K)

Show Material materials with Thermal conductivity of 27 - 27.3 W/(m·K)

500.0 °C

27.7 - 28 W/(m·K)

Show Material materials with Thermal conductivity of 27.7 - 28 W/(m·K)

600.0 °C

27.8 - 28 W/(m·K)

Show Material materials with Thermal conductivity of 27.8 - 28 W/(m·K)

700.0 °C

27.5 W/(m·K)

Show Material materials with Thermal conductivity of 27.5 W/(m·K)

Unlock all property charts

Thermal diffusivity

20.0 °C

5.7 mm²/s

Show Material materials with Thermal diffusivity of 5.7 mm²/s

100.0 °C

5.9 mm²/s

Show Material materials with Thermal diffusivity of 5.9 mm²/s

200.0 °C

6.1 mm²/s

Show Material materials with Thermal diffusivity of 6.1 mm²/s

300.0 °C

6 mm²/s

Show Material materials with Thermal diffusivity of 6 mm²/s

400.0 °C

5.8 mm²/s

Show Material materials with Thermal diffusivity of 5.8 mm²/s

500.0 °C

5.4 mm²/s

Show Material materials with Thermal diffusivity of 5.4 mm²/s

600.0 °C

4.7 mm²/s

Show Material materials with Thermal diffusivity of 4.7 mm²/s

Unlock all property charts

Electrical

PropertyTemperatureValue

Electrical resistivity

20.0 °C

5.14E-7 Ω·m

Show Material materials with Electrical resistivity of 5.14E-7 Ω·m

100.0 °C

5.6E-7 - 5.63E-7 Ω·m

Show Material materials with Electrical resistivity of 5.6E-7 - 5.63E-7 Ω·m

200.0 °C

6.3E-7 - 6.32E-7 Ω·m

Show Material materials with Electrical resistivity of 6.3E-7 - 6.32E-7 Ω·m

300.0 °C

7.1E-7 - 7.12E-7 Ω·m

Show Material materials with Electrical resistivity of 7.1E-7 - 7.12E-7 Ω·m

400.0 °C

7.97E-7 - 8E-7 Ω·m

Show Material materials with Electrical resistivity of 7.97E-7 - 8E-7 Ω·m

500.0 °C

8.9E-7 - 8.93E-7 Ω·m

Show Material materials with Electrical resistivity of 8.9E-7 - 8.93E-7 Ω·m

600.0 °C

9.96E-7 - 1E-6 Ω·m

Show Material materials with Electrical resistivity of 9.96E-7 - 1E-6 Ω·m

700.0 °C

1.12E-6 Ω·m

Show Material materials with Electrical resistivity of 1.12E-6 Ω·m

Unlock all property charts

Chemical properties

PropertyValue

Carbon

0.08 - 0.15 %

Show Material materials with Carbon of 0.08 - 0.15 %

Chromium

4 - 6 %

Show Material materials with Chromium of 4 - 6 %

Manganese

0.3 - 60 %

Show Material materials with Manganese of 0.3 - 60 %

Molybdenum

0.45 - 0.65 %

Show Material materials with Molybdenum of 0.45 - 0.65 %

Phosphorus

0.03 - 0.04 %

Show Material materials with Phosphorus of 0.03 - 0.04 %

Silicon

0.3 - 0.5 %

Show Material materials with Silicon of 0.3 - 0.5 %

Sulfur

0.03 - 0.035 %

Show Material materials with Sulfur of 0.03 - 0.035 %