General
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Density | 20 °C | 7.84 g/cm³ Show Material materials with Density of 7.84 g/cm³ | quenched and tempered (+QT) | EN 10028-2 | Sheet, Flat |
Mechanical
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Elastic modulus | -100 °C | 217 GPa Show Material materials with Elastic modulus of 217 GPa | quenched and tempered (+QT) | EN 10028-2 | Sheet, Flat | |
20 °C | 212 GPa Show Material materials with Elastic modulus of 212 GPa | quenched and tempered (+QT) | EN 10028-2 | Sheet, Flat | ||
100 °C | 207 GPa Show Material materials with Elastic modulus of 207 GPa | quenched and tempered (+QT) | EN 10028-2 | Sheet, Flat | ||
200 °C | 199 GPa Show Material materials with Elastic modulus of 199 GPa | quenched and tempered (+QT) | EN 10028-2 | Sheet, Flat | ||
300 °C | 192 GPa Show Material materials with Elastic modulus of 192 GPa | quenched and tempered (+QT) | EN 10028-2 | Sheet, Flat | ||
400 °C | 184 GPa Show Material materials with Elastic modulus of 184 GPa | quenched and tempered (+QT) | EN 10028-2 | Sheet, Flat | ||
500 °C | 175 GPa Show Material materials with Elastic modulus of 175 GPa | quenched and tempered (+QT) | EN 10028-2 | Sheet, Flat | ||
600 °C | 164 GPa Show Material materials with Elastic modulus of 164 GPa | quenched and tempered (+QT) | EN 10028-2 | Sheet, Flat | ||
Elongation | 15.1 % Show Material materials with Elongation of 15.1 % | Predicted Value, A200 | ||||
16.2 % Show Material materials with Elongation of 16.2 % | Predicted Value, A80 | |||||
16.8 % Show Material materials with Elongation of 16.8 % | Predicted Value, A80 Transverse | |||||
18.0 % Show Material materials with Elongation of 18.0 % | Predicted Value, A5 | |||||
19.4 % Show Material materials with Elongation of 19.4 % | Predicted Value, A50 | |||||
20 °C | 18 % Show Material materials with Elongation of 18 % | quenched and tempered (+QT) | EN 10028-2 | Flat, Sheet | Transverse | |
Hardness, Brinell | 231 [-] Show Material materials with Hardness, Brinell of 231 [-] | Predicted Value, Transverse | ||||
Poisson's ratio | 0.29 [-] Show Material materials with Poisson's ratio of 0.29 [-] | Typical for Chromium Molybdenum Steel | ||||
Reduction of area | 20 °C | 50 % Show Material materials with Reduction of area of 50 % | quenched and tempered (+QT) | EN 10028-2 | Sheet | Transverse |
Shear modulus | 81.1 GPa Show Material materials with Shear modulus of 81.1 GPa | Predicted Value | ||||
Shear strength | 669.4 MPa Show Material materials with Shear strength of 669.4 MPa | Predicted Value | ||||
Tensile strength | 20 °C | 520 - 690 MPa Show Material materials with Tensile strength of 520 - 690 MPa | quenched and tempered (+QT) | EN 10028-2 | Sheet | Transverse |
20 °C | 520 - 670 MPa Show Material materials with Tensile strength of 520 - 670 MPa | quenched and tempered (+QT) | EN 10028-2 | Sheet | Transverse | |
20 °C | 540 - 690 MPa Show Material materials with Tensile strength of 540 - 690 MPa | quenched and tempered (+QT) | EN 10028-2 | Flat, Sheet | Transverse | |
20 °C | 540 - 670 MPa Show Material materials with Tensile strength of 540 - 670 MPa | quenched and tempered (+QT) | EN 10028-2 | Sheet | Transverse | |
Yield strength | 247.1 MPa Show Material materials with Yield strength of 247.1 MPa | Predicted Value, RP1 Transverse | ||||
275.1 MPa Show Material materials with Yield strength of 275.1 MPa | Predicted Value, RP1 | |||||
376.1 MPa Show Material materials with Yield strength of 376.1 MPa | Predicted Value, Transverse | |||||
388 MPa Show Material materials with Yield strength of 388 MPa | Predicted Value, RP05 | |||||
614.7 MPa Show Material materials with Yield strength of 614.7 MPa | Predicted Value, RP002 | |||||
20 °C | 330 MPa Show Material materials with Yield strength of 330 MPa | quenched and tempered (+QT) | EN 10028-2 | Sheet | RP02 Transverse | |
20 °C | 355 MPa Show Material materials with Yield strength of 355 MPa | quenched and tempered (+QT) | EN 10028-2 | Flat, Sheet | RP02 Transverse | |
50 °C | 341 MPa Show Material materials with Yield strength of 341 MPa | quenched and tempered (+QT) | EN 10028-2 | Flat | RP02 | |
100 °C | 320 MPa Show Material materials with Yield strength of 320 MPa | quenched and tempered (+QT) | EN 10028-2 | Sheet | RP02 Transverse | |
100 °C | 323 MPa Show Material materials with Yield strength of 323 MPa | quenched and tempered (+QT) | EN 10028-2 | Flat | RP02 | |
100 °C | 338 MPa Show Material materials with Yield strength of 338 MPa | quenched and tempered (+QT) | EN 10028-2 | Sheet | RP02 Transverse | |
150 °C | 311 MPa Show Material materials with Yield strength of 311 MPa | quenched and tempered (+QT) | EN 10028-2 | Flat | RP02 | |
200 °C | 300 MPa Show Material materials with Yield strength of 300 MPa | quenched and tempered (+QT) | EN 10028-2 | Sheet | RP02 Transverse | |
200 °C | 303 MPa Show Material materials with Yield strength of 303 MPa | quenched and tempered (+QT) | EN 10028-2 | Flat | RP02 | |
200 °C | 319 MPa Show Material materials with Yield strength of 319 MPa | quenched and tempered (+QT) | EN 10028-2 | Sheet | RP02 Transverse | |
250 °C | 280 MPa Show Material materials with Yield strength of 280 MPa | quenched and tempered (+QT) | EN 10028-2 | Sheet | RP02 Transverse | |
250 °C | 298 MPa Show Material materials with Yield strength of 298 MPa | quenched and tempered (+QT) | EN 10028-2 | Flat | RP02 | |
250 °C | 309 MPa Show Material materials with Yield strength of 309 MPa | quenched and tempered (+QT) | EN 10028-2 | Sheet | RP02 Transverse | |
300 °C | 275 MPa Show Material materials with Yield strength of 275 MPa | quenched and tempered (+QT) | EN 10028-2 | Sheet | RP02 Transverse | |
300 °C | 295 MPa Show Material materials with Yield strength of 295 MPa | quenched and tempered (+QT) | EN 10028-2 | Flat | RP02 | |
300 °C | 304 MPa Show Material materials with Yield strength of 304 MPa | quenched and tempered (+QT) | EN 10028-2 | Sheet | RP02 Transverse | |
350 °C | 270 MPa Show Material materials with Yield strength of 270 MPa | quenched and tempered (+QT) | EN 10028-2 | Sheet | RP02 Transverse | |
350 °C | 292 MPa Show Material materials with Yield strength of 292 MPa | quenched and tempered (+QT) | EN 10028-2 | Flat | RP02 | |
350 °C | 294 MPa Show Material materials with Yield strength of 294 MPa | quenched and tempered (+QT) | EN 10028-2 | Sheet | RP02 Transverse | |
400 °C | 260 MPa Show Material materials with Yield strength of 260 MPa | quenched and tempered (+QT) | EN 10028-2 | Sheet | RP02 Transverse | |
400 °C | 284 MPa Show Material materials with Yield strength of 284 MPa | quenched and tempered (+QT) | EN 10028-2 | Sheet | RP02 Transverse | |
400 °C | 287 MPa Show Material materials with Yield strength of 287 MPa | quenched and tempered (+QT) | EN 10028-2 | Sheet | RP02 Transverse | |
400 °C | 287 MPa Show Material materials with Yield strength of 287 MPa | quenched and tempered (+QT) | EN 10028-2 | Flat | RP02 | |
450 °C | 250 MPa Show Material materials with Yield strength of 250 MPa | quenched and tempered (+QT) | EN 10028-2 | Sheet | RP02 Transverse | |
450 °C | 275 MPa Show Material materials with Yield strength of 275 MPa | quenched and tempered (+QT) | EN 10028-2 | Sheet | RP02 Transverse | |
450 °C | 279 MPa Show Material materials with Yield strength of 279 MPa | quenched and tempered (+QT) | EN 10028-2 | Sheet | RP02 Transverse | |
450 °C | 279 MPa Show Material materials with Yield strength of 279 MPa | quenched and tempered (+QT) | EN 10028-2 | Flat | RP02 |
Thermal
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Coefficient of thermal expansion | -100 °C | 1.05e-05 1/K Show Material materials with Coefficient of thermal expansion of 1.05e-05 1/K | quenched and tempered (+QT) | EN 10028-2 | Sheet, Flat | |
20 °C | 1.15e-05 1/K Show Material materials with Coefficient of thermal expansion of 1.15e-05 1/K | quenched and tempered (+QT) | EN 10028-2 | Sheet, Flat | ||
100 °C | 1.21e-05 1/K Show Material materials with Coefficient of thermal expansion of 1.21e-05 1/K | quenched and tempered (+QT) | EN 10028-2 | Sheet, Flat | ||
200 °C | 1.27e-05 1/K Show Material materials with Coefficient of thermal expansion of 1.27e-05 1/K | quenched and tempered (+QT) | EN 10028-2 | Sheet, Flat | ||
300 °C | 1.32e-05 1/K Show Material materials with Coefficient of thermal expansion of 1.32e-05 1/K | quenched and tempered (+QT) | EN 10028-2 | Sheet, Flat | ||
400 °C | 1.36e-05 1/K Show Material materials with Coefficient of thermal expansion of 1.36e-05 1/K | quenched and tempered (+QT) | EN 10028-2 | Sheet, Flat | ||
500 °C | 1.4e-05 1/K Show Material materials with Coefficient of thermal expansion of 1.4e-05 1/K | quenched and tempered (+QT) | EN 10028-2 | Sheet, Flat | ||
600 °C | 1.44e-05 1/K Show Material materials with Coefficient of thermal expansion of 1.44e-05 1/K | quenched and tempered (+QT) | EN 10028-2 | Sheet, Flat | ||
Max service temperature | 20 - 450 °C Show Material materials with Max service temperature of 20 - 450 °C | quenched and tempered (+QT) | EN 10028-2 | Flat | Long | |
Melting point | 1382 - 1529 °C Show Material materials with Melting point of 1382 - 1529 °C | Typical for Chromium Molybdenum Steel | ||||
Specific heat capacity | -100 °C | 423 J/(kg·K) Show Material materials with Specific heat capacity of 423 J/(kg·K) | quenched and tempered (+QT) | EN 10028-2 | Sheet, Flat | |
20 °C | 461 J/(kg·K) Show Material materials with Specific heat capacity of 461 J/(kg·K) | quenched and tempered (+QT) | EN 10028-2 | Sheet, Flat | ||
100 °C | 479 J/(kg·K) Show Material materials with Specific heat capacity of 479 J/(kg·K) | quenched and tempered (+QT) | EN 10028-2 | Sheet, Flat | ||
200 °C | 499 J/(kg·K) Show Material materials with Specific heat capacity of 499 J/(kg·K) | quenched and tempered (+QT) | EN 10028-2 | Sheet, Flat | ||
300 °C | 517 J/(kg·K) Show Material materials with Specific heat capacity of 517 J/(kg·K) | quenched and tempered (+QT) | EN 10028-2 | Sheet, Flat | ||
400 °C | 536 J/(kg·K) Show Material materials with Specific heat capacity of 536 J/(kg·K) | quenched and tempered (+QT) | EN 10028-2 | Sheet, Flat | ||
500 °C | 558 J/(kg·K) Show Material materials with Specific heat capacity of 558 J/(kg·K) | quenched and tempered (+QT) | EN 10028-2 | Sheet, Flat | ||
600 °C | 587 J/(kg·K) Show Material materials with Specific heat capacity of 587 J/(kg·K) | quenched and tempered (+QT) | EN 10028-2 | Sheet, Flat | ||
Thermal conductivity | 20 °C | 34.9 W/(m·K) Show Material materials with Thermal conductivity of 34.9 W/(m·K) | quenched and tempered (+QT) | EN 10028-2 | Sheet, Flat | |
100 °C | 37.3 W/(m·K) Show Material materials with Thermal conductivity of 37.3 W/(m·K) | quenched and tempered (+QT) | EN 10028-2 | Sheet, Flat | ||
200 °C | 38.2 W/(m·K) Show Material materials with Thermal conductivity of 38.2 W/(m·K) | quenched and tempered (+QT) | EN 10028-2 | Sheet, Flat | ||
300 °C | 37.8 W/(m·K) Show Material materials with Thermal conductivity of 37.8 W/(m·K) | quenched and tempered (+QT) | EN 10028-2 | Sheet, Flat | ||
400 °C | 36.6 W/(m·K) Show Material materials with Thermal conductivity of 36.6 W/(m·K) | quenched and tempered (+QT) | EN 10028-2 | Sheet, Flat | ||
500 °C | 35.2 W/(m·K) Show Material materials with Thermal conductivity of 35.2 W/(m·K) | quenched and tempered (+QT) | EN 10028-2 | Sheet, Flat | ||
600 °C | 33.6 W/(m·K) Show Material materials with Thermal conductivity of 33.6 W/(m·K) | quenched and tempered (+QT) | EN 10028-2 | Sheet, Flat | ||
Thermal diffusivity | 20 °C | 9.7 mm²/s Show Material materials with Thermal diffusivity of 9.7 mm²/s | quenched and tempered (+QT) | EN 10028-2 | Sheet, Flat | |
100 °C | 9.6 mm²/s Show Material materials with Thermal diffusivity of 9.6 mm²/s | quenched and tempered (+QT) | EN 10028-2 | Sheet, Flat | ||
200 °C | 9.2 mm²/s Show Material materials with Thermal diffusivity of 9.2 mm²/s | quenched and tempered (+QT) | EN 10028-2 | Sheet, Flat | ||
300 °C | 8.5 mm²/s Show Material materials with Thermal diffusivity of 8.5 mm²/s | quenched and tempered (+QT) | EN 10028-2 | Sheet, Flat | ||
400 °C | 7.8 mm²/s Show Material materials with Thermal diffusivity of 7.8 mm²/s | quenched and tempered (+QT) | EN 10028-2 | Sheet, Flat | ||
500 °C | 6.8 mm²/s Show Material materials with Thermal diffusivity of 6.8 mm²/s | quenched and tempered (+QT) | EN 10028-2 | Sheet, Flat | ||
600 °C | 5.7 mm²/s Show Material materials with Thermal diffusivity of 5.7 mm²/s | quenched and tempered (+QT) | EN 10028-2 | Sheet, Flat |
Electrical
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Electrical conductivity | 3 S/m Show Material materials with Electrical conductivity of 3 S/m | Predicted Value | ||||
Electrical resistivity | 20 °C | 2.98e-07 Ω·m Show Material materials with Electrical resistivity of 2.98e-07 Ω·m | quenched and tempered (+QT) | EN 10028-2 | Sheet, Flat | |
100 °C | 3.43e-07 Ω·m Show Material materials with Electrical resistivity of 3.43e-07 Ω·m | quenched and tempered (+QT) | EN 10028-2 | Sheet, Flat | ||
200 °C | 4.13e-07 Ω·m Show Material materials with Electrical resistivity of 4.13e-07 Ω·m | quenched and tempered (+QT) | EN 10028-2 | Sheet, Flat | ||
300 °C | 4.97e-07 Ω·m Show Material materials with Electrical resistivity of 4.97e-07 Ω·m | quenched and tempered (+QT) | EN 10028-2 | Sheet, Flat | ||
400 °C | 5.95e-07 Ω·m Show Material materials with Electrical resistivity of 5.95e-07 Ω·m | quenched and tempered (+QT) | EN 10028-2 | Sheet, Flat | ||
500 °C | 7.03e-07 Ω·m Show Material materials with Electrical resistivity of 7.03e-07 Ω·m | quenched and tempered (+QT) | EN 10028-2 | Sheet, Flat | ||
600 °C | 8.25e-07 Ω·m Show Material materials with Electrical resistivity of 8.25e-07 Ω·m | quenched and tempered (+QT) | EN 10028-2 | Sheet, Flat |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Aluminium | 0.01 - 0.04 % Show Material materials with Aluminium of 0.01 - 0.04 % | quenched and tempered (+QT) | EN 10028-2 | Sheet, Flat |
0.01 - 0.035 % Show Material materials with Aluminium of 0.01 - 0.035 % | quenched and tempered (+QT) | EN 10028-2 | Sheet | |
Carbon | 0.1 - 0.15 % Show Material materials with Carbon of 0.1 - 0.15 % | quenched and tempered (+QT) | EN 10028-2 | Sheet, Flat |
Chromium | 2 - 2.5 % Show Material materials with Chromium of 2 - 2.5 % | quenched and tempered (+QT) | EN 10028-2 | Sheet, Flat |
Copper | 0.2 % Show Material materials with Copper of 0.2 % | quenched and tempered (+QT) | EN 10028-2 | Sheet |
0.25 % Show Material materials with Copper of 0.25 % | quenched and tempered (+QT) | EN 10028-2 | Sheet, Flat | |
Manganese | 0.3 - 0.8 % Show Material materials with Manganese of 0.3 - 0.8 % | quenched and tempered (+QT) | EN 10028-2 | Sheet, Flat |
Molybdenum | 0.9 - 1.1 % Show Material materials with Molybdenum of 0.9 - 1.1 % | quenched and tempered (+QT) | EN 10028-2 | Sheet, Flat |
Nickel | 0.3 % Show Material materials with Nickel of 0.3 % | quenched and tempered (+QT) | EN 10028-2 | Sheet, Flat |
Nitrogen | 0.012 % Show Material materials with Nitrogen of 0.012 % | quenched and tempered (+QT) | EN 10028-2 | Sheet, Flat |
Phosphorus | 0.015 % Show Material materials with Phosphorus of 0.015 % | quenched and tempered (+QT) | EN 10028-2 | Sheet, Flat |
Silicon | 0.3 % Show Material materials with Silicon of 0.3 % | quenched and tempered (+QT) | EN 10028-2 | Sheet, Flat |
Sulfur | 0.01 % Show Material materials with Sulfur of 0.01 % | quenched and tempered (+QT) | EN 10028-2 | Sheet, Flat |
0.012 % Show Material materials with Sulfur of 0.012 % | quenched and tempered (+QT) | EN 10028-2 | Sheet |
Technological properties
Property | ||
---|---|---|
Supplier Disclaimer | The given information is a rough description and some properties can depend on various factors such as product thickness. Please contact the supplier or refer to the related norm or standard for further information. |