General
Property | Temperature | Value |
---|---|---|
Density | 20.0 °C | 7.83 g/cm³ Show Material materials with Density of 7.83 g/cm³ |
Mechanical
Property | Temperature | Value | Comment |
---|---|---|---|
Elastic modulus | -100.0 °C | 217 GPa Show Material materials with Elastic modulus of 217 GPa | |
20.0 °C | 212 GPa Show Material materials with Elastic modulus of 212 GPa | ||
100.0 °C | 207 - 209 GPa Show Material materials with Elastic modulus of 207 - 209 GPa | ||
200.0 °C | 199 - 202 GPa Show Material materials with Elastic modulus of 199 - 202 GPa | ||
300.0 °C | 192 - 195 GPa Show Material materials with Elastic modulus of 192 - 195 GPa | ||
400.0 °C | 184 - 187 GPa Show Material materials with Elastic modulus of 184 - 187 GPa | ||
500.0 °C | 175 - 178 GPa Show Material materials with Elastic modulus of 175 - 178 GPa | ||
600.0 °C | 164 - 167 GPa Show Material materials with Elastic modulus of 164 - 167 GPa | ||
Elongation | 20.0 °C | 17 % Show Material materials with Elongation of 17 % | |
Elongation, transverse | 20.0 °C | 13 % Show Material materials with Elongation, transverse of 13 % | |
Poisson's ratio | 23.0 °C | 0.29 [-] Show Material materials with Poisson's ratio of 0.29 [-] | Typical for Chromium Molybdenum Steel |
Tensile strength | 20.0 °C | 740 - 880 MPa Show Material materials with Tensile strength of 740 - 880 MPa | |
100.0 °C | 690 MPa Show Material materials with Tensile strength of 690 MPa | ||
150.0 °C | 670 MPa Show Material materials with Tensile strength of 670 MPa | ||
200.0 °C | 650 MPa Show Material materials with Tensile strength of 650 MPa | ||
250.0 °C | 630 MPa Show Material materials with Tensile strength of 630 MPa | ||
300.0 °C | 610 MPa Show Material materials with Tensile strength of 610 MPa | ||
350.0 °C | 570 MPa Show Material materials with Tensile strength of 570 MPa | ||
400.0 °C | 520 MPa Show Material materials with Tensile strength of 520 MPa | ||
450.0 °C | 465 MPa Show Material materials with Tensile strength of 465 MPa | ||
500.0 °C | 410 MPa Show Material materials with Tensile strength of 410 MPa | ||
Tensile strength, transverse | 20.0 °C | 740 - 880 MPa Show Material materials with Tensile strength, transverse of 740 - 880 MPa | |
Yield strength Rp0.2 | 20.0 °C | 590 MPa Show Material materials with Yield strength Rp0.2 of 590 MPa | |
100.0 °C | 580 MPa Show Material materials with Yield strength Rp0.2 of 580 MPa | ||
150.0 °C | 575 MPa Show Material materials with Yield strength Rp0.2 of 575 MPa | ||
200.0 °C | 570 MPa Show Material materials with Yield strength Rp0.2 of 570 MPa | ||
250.0 °C | 560 MPa Show Material materials with Yield strength Rp0.2 of 560 MPa | ||
300.0 °C | 530 MPa Show Material materials with Yield strength Rp0.2 of 530 MPa | ||
350.0 °C | 510 MPa Show Material materials with Yield strength Rp0.2 of 510 MPa | ||
400.0 °C | 470 MPa Show Material materials with Yield strength Rp0.2 of 470 MPa | ||
450.0 °C | 420 MPa Show Material materials with Yield strength Rp0.2 of 420 MPa | ||
500.0 °C | 370 MPa Show Material materials with Yield strength Rp0.2 of 370 MPa | ||
Yield strength Rp0.2, transverse | 20.0 °C | 590 MPa Show Material materials with Yield strength Rp0.2, transverse of 590 MPa |
Thermal
Property | Temperature | Value | Comment |
---|---|---|---|
Coefficient of thermal expansion | -100.0 °C | 1.05E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.05E-5 1/K | |
20.0 °C | 1.15E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.15E-5 1/K | ||
100.0 °C | 1.19E-5 - 1.21E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.19E-5 - 1.21E-5 1/K | ||
200.0 °C | 1.25E-5 - 1.27E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.25E-5 - 1.27E-5 1/K | ||
300.0 °C | 1.3E-5 - 1.32E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.3E-5 - 1.32E-5 1/K | ||
400.0 °C | 1.34E-5 - 1.36E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.34E-5 - 1.36E-5 1/K | ||
500.0 °C | 1.38E-5 - 1.4E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.38E-5 - 1.4E-5 1/K | ||
600.0 °C | 1.41E-5 - 1.44E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.41E-5 - 1.44E-5 1/K | ||
Max service temperature, long | 0 - 480 °C Show Material materials with Max service temperature, long of 0 - 480 °C | ||
Melting point | 1382 - 1529 °C Show Material materials with Melting point of 1382 - 1529 °C | Typical for Chromium Molybdenum Steel | |
Specific heat capacity | -100.0 °C | 423 J/(kg·K) Show Material materials with Specific heat capacity of 423 J/(kg·K) | |
20.0 °C | 461 J/(kg·K) Show Material materials with Specific heat capacity of 461 J/(kg·K) | ||
100.0 °C | 460 - 479 J/(kg·K) Show Material materials with Specific heat capacity of 460 - 479 J/(kg·K) | ||
200.0 °C | 480 - 499 J/(kg·K) Show Material materials with Specific heat capacity of 480 - 499 J/(kg·K) | ||
300.0 °C | 500 - 517 J/(kg·K) Show Material materials with Specific heat capacity of 500 - 517 J/(kg·K) | ||
400.0 °C | 520 - 536 J/(kg·K) Show Material materials with Specific heat capacity of 520 - 536 J/(kg·K) | ||
500.0 °C | 550 - 558 J/(kg·K) Show Material materials with Specific heat capacity of 550 - 558 J/(kg·K) | ||
600.0 °C | 570 - 587 J/(kg·K) Show Material materials with Specific heat capacity of 570 - 587 J/(kg·K) | ||
Thermal conductivity | 20.0 °C | 25.7 W/(m·K) Show Material materials with Thermal conductivity of 25.7 W/(m·K) | |
100.0 °C | 27 - 27.4 W/(m·K) Show Material materials with Thermal conductivity of 27 - 27.4 W/(m·K) | ||
200.0 °C | 28.5 - 29 W/(m·K) Show Material materials with Thermal conductivity of 28.5 - 29 W/(m·K) | ||
300.0 °C | 28.9 - 29 W/(m·K) Show Material materials with Thermal conductivity of 28.9 - 29 W/(m·K) | ||
400.0 °C | 28.5 - 29 W/(m·K) Show Material materials with Thermal conductivity of 28.5 - 29 W/(m·K) | ||
500.0 °C | 27.7 - 28 W/(m·K) Show Material materials with Thermal conductivity of 27.7 - 28 W/(m·K) | ||
600.0 °C | 26.8 - 27 W/(m·K) Show Material materials with Thermal conductivity of 26.8 - 27 W/(m·K) | ||
Thermal diffusivity | 20.0 °C | 7.1 mm²/s Show Material materials with Thermal diffusivity of 7.1 mm²/s | |
100.0 °C | 7.1 mm²/s Show Material materials with Thermal diffusivity of 7.1 mm²/s | ||
200.0 °C | 6.9 mm²/s Show Material materials with Thermal diffusivity of 6.9 mm²/s | ||
300.0 °C | 6.6 mm²/s Show Material materials with Thermal diffusivity of 6.6 mm²/s | ||
400.0 °C | 6.1 mm²/s Show Material materials with Thermal diffusivity of 6.1 mm²/s | ||
500.0 °C | 5.3 mm²/s Show Material materials with Thermal diffusivity of 5.3 mm²/s | ||
600.0 °C | 4.5 mm²/s Show Material materials with Thermal diffusivity of 4.5 mm²/s | ||
Electrical
Property | Temperature | Value |
---|---|---|
Electrical resistivity | 20.0 °C | 4.05E-7 Ω·m Show Material materials with Electrical resistivity of 4.05E-7 Ω·m |
100.0 °C | 4.67E-7 - 4.7E-7 Ω·m Show Material materials with Electrical resistivity of 4.67E-7 - 4.7E-7 Ω·m | |
200.0 °C | 5.5E-7 - 5.53E-7 Ω·m Show Material materials with Electrical resistivity of 5.5E-7 - 5.53E-7 Ω·m | |
300.0 °C | 6.5E-7 Ω·m Show Material materials with Electrical resistivity of 6.5E-7 Ω·m | |
400.0 °C | 7.6E-7 - 7.62E-7 Ω·m Show Material materials with Electrical resistivity of 7.6E-7 - 7.62E-7 Ω·m | |
500.0 °C | 8.9E-7 - 8.92E-7 Ω·m Show Material materials with Electrical resistivity of 8.9E-7 - 8.92E-7 Ω·m | |
600.0 °C | 1.03E-6 Ω·m Show Material materials with Electrical resistivity of 1.03E-6 Ω·m | |
Chemical properties
Property | Value |
---|---|
Carbon | 0.17 - 0.23 % Show Material materials with Carbon of 0.17 - 0.23 % |
Chromium | 3 - 3.3 % Show Material materials with Chromium of 3 - 3.3 % |
Manganese | 0.3 - 0.5 % Show Material materials with Manganese of 0.3 - 0.5 % |
Molybdenum | 0.5 - 0.6 % Show Material materials with Molybdenum of 0.5 - 0.6 % |
Phosphorus | 0.02 % Show Material materials with Phosphorus of 0.02 % |
Silicon | 0.15 - 0.35 % Show Material materials with Silicon of 0.15 - 0.35 % |
Sulfur | 0.02 % Show Material materials with Sulfur of 0.02 % |
Vanadium | 0.45 - 0.55 % Show Material materials with Vanadium of 0.45 - 0.55 % |