DIN 17205 Grade GS-30Mn5 air quenched and tempered

View suppliers (1)
Want to keep this datasheet? Save it now in your required format

Description

The material GS-30 Mn 5 is applicable up to 300 degrees C. The use is performed in the construction of cranes and conveyor systems, in the vehicle and gear manufacturing as well as in the general mechanical engineering, e.g. for impellers, ball races, bearing rollers, drive tumblers, cog wheels, toothed rims.

Related Standards

Equivalent Materials

This material data has been provided by WIAM.

"Typical" values were obtained via a literature search. "Predicted" values were imputed via artificial intelligence technology. While we have placed significant efforts in ensuring data accuracy, "typical" and "predicted" data should be considered indicative and verified by appropriate material testing. Please do contact us if additional information on the the predicted data method is required.
All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValue

Density

20.0 °C

7.85 g/cm³

Show Material materials with Density of 7.85 g/cm³

Mechanical

PropertyTemperatureValueComment

Elastic modulus

20.0 °C

211 GPa

Show Material materials with Elastic modulus of 211 GPa

100.0 °C

204 GPa

Show Material materials with Elastic modulus of 204 GPa

200.0 °C

196 GPa

Show Material materials with Elastic modulus of 196 GPa

300.0 °C

186 GPa

Show Material materials with Elastic modulus of 186 GPa

Elongation

20.0 °C

18 %

Show Material materials with Elongation of 18 %

Poisson's ratio

23.0 °C

0.29 [-]

Show Material materials with Poisson's ratio of 0.29 [-]

Typical for Medium Carbon Steel

Shear modulus

23.0 °C

75 - 80 GPa

Show Material materials with Shear modulus of 75 - 80 GPa

Typical for Carbon Steel

Tensile strength

20.0 °C

520 - 670 MPa

Show Material materials with Tensile strength of 520 - 670 MPa

Yield strength Rp0.2

20.0 °C

260 MPa

Show Material materials with Yield strength Rp0.2 of 260 MPa

Thermal

PropertyTemperatureValueComment

Coefficient of thermal expansion

100.0 °C

1.1E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.1E-5 1/K

200.0 °C

1.2E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.2E-5 1/K

300.0 °C

1.3E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.3E-5 1/K

Unlock all property charts

Max service temperature

500 °C

Show Material materials with Max service temperature of 500 °C

Typical for Carbon Steel

Max service temperature, long

0 - 300 °C

Show Material materials with Max service temperature, long of 0 - 300 °C

Melting point

1380 - 1514 °C

Show Material materials with Melting point of 1380 - 1514 °C

Typical for Medium Carbon Steel

Specific heat capacity

23.0 °C

470 - 520 J/(kg·K)

Show Material materials with Specific heat capacity of 470 - 520 J/(kg·K)

Typical for Medium Carbon Steel

Thermal conductivity

23.0 °C

21 - 52 W/(m·K)

Show Material materials with Thermal conductivity of 21 - 52 W/(m·K)

Typical for Medium Carbon Steel

Electrical

PropertyTemperatureValueComment

Electrical resistivity

23.0 °C

1.43E-7 - 1.74E-7 Ω·m

Show Material materials with Electrical resistivity of 1.43E-7 - 1.74E-7 Ω·m

Typical for Carbon Steel

Chemical properties

PropertyValue

Carbon

0.27 - 0.34 %

Show Material materials with Carbon of 0.27 - 0.34 %

Manganese

1.2 - 1.5 %

Show Material materials with Manganese of 1.2 - 1.5 %

Phosphorus

0.02 %

Show Material materials with Phosphorus of 0.02 %

Silicon

0.6 %

Show Material materials with Silicon of 0.6 %

Sulfur

0.015 %

Show Material materials with Sulfur of 0.015 %

Do you have a technical question or need more information about this material?