General
Property | Temperature | Value |
---|---|---|
Density | 20.0 °C | 7.78 g/cm³ Show Material materials with Density of 7.78 g/cm³ |
Mechanical
Property | Temperature | Value | Comment |
---|---|---|---|
Elastic modulus | -100.0 °C | 217 GPa Show Material materials with Elastic modulus of 217 GPa | |
20.0 °C | 206 - 212 GPa Show Material materials with Elastic modulus of 206 - 212 GPa | ||
100.0 °C | 207 GPa Show Material materials with Elastic modulus of 207 GPa | ||
200.0 °C | 199 GPa Show Material materials with Elastic modulus of 199 GPa | ||
300.0 °C | 192 GPa Show Material materials with Elastic modulus of 192 GPa | ||
400.0 °C | 184 GPa Show Material materials with Elastic modulus of 184 GPa | ||
500.0 °C | 175 GPa Show Material materials with Elastic modulus of 175 GPa | ||
600.0 °C | 164 GPa Show Material materials with Elastic modulus of 164 GPa | ||
Hardness, Vickers | 20.0 °C | 680 [-] Show Material materials with Hardness, Vickers of 680 [-] | |
Poisson's ratio | 23.0 °C | 0.3 [-] Show Material materials with Poisson's ratio of 0.3 [-] | Typical for Steel |
Shear modulus | 20.0 °C | 78 GPa Show Material materials with Shear modulus of 78 GPa |
Thermal
Property | Temperature | Value |
---|---|---|
Coefficient of thermal expansion | -100.0 °C | 1.05E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.05E-5 1/K |
20.0 °C | 1.15E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.15E-5 1/K | |
100.0 °C | 1.21E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.21E-5 1/K | |
200.0 °C | 1.27E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.27E-5 1/K | |
300.0 °C | 1.32E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.32E-5 1/K | |
400.0 °C | 1.36E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.36E-5 1/K | |
500.0 °C | 1.4E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.4E-5 1/K | |
600.0 °C | 1.44E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.44E-5 1/K | |
Specific heat capacity | 20.0 °C | 461 J/(kg·K) Show Material materials with Specific heat capacity of 461 J/(kg·K) |
100.0 °C | 479 J/(kg·K) Show Material materials with Specific heat capacity of 479 J/(kg·K) | |
200.0 °C | 499 J/(kg·K) Show Material materials with Specific heat capacity of 499 J/(kg·K) | |
300.0 °C | 517 J/(kg·K) Show Material materials with Specific heat capacity of 517 J/(kg·K) | |
400.0 °C | 536 J/(kg·K) Show Material materials with Specific heat capacity of 536 J/(kg·K) | |
500.0 °C | 558 J/(kg·K) Show Material materials with Specific heat capacity of 558 J/(kg·K) | |
600.0 °C | 587 J/(kg·K) Show Material materials with Specific heat capacity of 587 J/(kg·K) | |
Thermal conductivity | 20.0 °C | 34.1 W/(m·K) Show Material materials with Thermal conductivity of 34.1 W/(m·K) |
100.0 °C | 35.2 W/(m·K) Show Material materials with Thermal conductivity of 35.2 W/(m·K) | |
200.0 °C | 36.5 W/(m·K) Show Material materials with Thermal conductivity of 36.5 W/(m·K) | |
300.0 °C | 36.7 W/(m·K) Show Material materials with Thermal conductivity of 36.7 W/(m·K) | |
400.0 °C | 35.8 W/(m·K) Show Material materials with Thermal conductivity of 35.8 W/(m·K) | |
500.0 °C | 34.5 W/(m·K) Show Material materials with Thermal conductivity of 34.5 W/(m·K) | |
600.0 °C | 32.9 W/(m·K) Show Material materials with Thermal conductivity of 32.9 W/(m·K) | |
Thermal diffusivity | 20.0 °C | 9.5 mm²/s Show Material materials with Thermal diffusivity of 9.5 mm²/s |
100.0 °C | 9.2 mm²/s Show Material materials with Thermal diffusivity of 9.2 mm²/s | |
200.0 °C | 8.9 mm²/s Show Material materials with Thermal diffusivity of 8.9 mm²/s | |
300.0 °C | 8.3 mm²/s Show Material materials with Thermal diffusivity of 8.3 mm²/s | |
400.0 °C | 7.7 mm²/s Show Material materials with Thermal diffusivity of 7.7 mm²/s | |
500.0 °C | 6.7 mm²/s Show Material materials with Thermal diffusivity of 6.7 mm²/s | |
600.0 °C | 5.6 mm²/s Show Material materials with Thermal diffusivity of 5.6 mm²/s | |
Electrical
Property | Temperature | Value |
---|---|---|
Electrical resistivity | 20.0 °C | 3.05E-7 Ω·m Show Material materials with Electrical resistivity of 3.05E-7 Ω·m |
100.0 °C | 3.64E-7 Ω·m Show Material materials with Electrical resistivity of 3.64E-7 Ω·m | |
200.0 °C | 4.32E-7 Ω·m Show Material materials with Electrical resistivity of 4.32E-7 Ω·m | |
300.0 °C | 5.12E-7 Ω·m Show Material materials with Electrical resistivity of 5.12E-7 Ω·m | |
400.0 °C | 6.07E-7 Ω·m Show Material materials with Electrical resistivity of 6.07E-7 Ω·m | |
500.0 °C | 7.16E-7 Ω·m Show Material materials with Electrical resistivity of 7.16E-7 Ω·m | |
600.0 °C | 8.42E-7 Ω·m Show Material materials with Electrical resistivity of 8.42E-7 Ω·m | |
Chemical properties
Property | Value |
---|---|
Carbon | 0.68 - 0.75 % Show Material materials with Carbon of 0.68 - 0.75 % |
Manganese | 0.6 - 0.8 % Show Material materials with Manganese of 0.6 - 0.8 % |
Phosphorus | 0.04 % Show Material materials with Phosphorus of 0.04 % |
Silicon | 1.5 - 1.8 % Show Material materials with Silicon of 1.5 - 1.8 % |
Sulfur | 0.035 % Show Material materials with Sulfur of 0.035 % |
Technological properties
Property | ||
---|---|---|
Features | Spring |
Do you have a technical question or need more information about this material?
Post it as a comment below and receive answers from engineers and other community members.