General
Property | Temperature | Value |
---|---|---|
Density | 20.0 °C | 7.8 - 7.85 g/cm³ Show Material materials with Density of 7.8 - 7.85 g/cm³ |
Mechanical
Property | Temperature | Value | Comment |
---|---|---|---|
Elastic modulus | -100.0 °C | 217 GPa Show Material materials with Elastic modulus of 217 GPa | |
20.0 °C | 212 GPa Show Material materials with Elastic modulus of 212 GPa | ||
100.0 °C | 207 GPa Show Material materials with Elastic modulus of 207 GPa | ||
200.0 °C | 199 GPa Show Material materials with Elastic modulus of 199 GPa | ||
300.0 °C | 192 GPa Show Material materials with Elastic modulus of 192 GPa | ||
400.0 °C | 184 GPa Show Material materials with Elastic modulus of 184 GPa | ||
500.0 °C | 175 GPa Show Material materials with Elastic modulus of 175 GPa | ||
600.0 °C | 164 GPa Show Material materials with Elastic modulus of 164 GPa | ||
Elongation | 20.0 °C | 12 - 15 % Show Material materials with Elongation of 12 - 15 % | |
Poisson's ratio | 23.0 °C | 0.3 [-] Show Material materials with Poisson's ratio of 0.3 [-] | Typical for Steel |
Reduction of area | 20.0 °C | 35 - 45 % Show Material materials with Reduction of area of 35 - 45 % | |
Tensile strength | 20.0 °C | 650 - 1100 MPa Show Material materials with Tensile strength of 650 - 1100 MPa | |
Yield strength | 20.0 °C | 400 - 650 MPa Show Material materials with Yield strength of 400 - 650 MPa |
Thermal
Property | Temperature | Value |
---|---|---|
Coefficient of thermal expansion | -100.0 °C | 1.08E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.08E-5 1/K |
20.0 °C | 1.19E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.19E-5 1/K | |
100.0 °C | 1.25E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.25E-5 1/K | |
200.0 °C | 1.3E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.3E-5 1/K | |
300.0 °C | 1.36E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.36E-5 1/K | |
400.0 °C | 1.41E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.41E-5 1/K | |
500.0 °C | 1.45E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.45E-5 1/K | |
600.0 °C | 1.49E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.49E-5 1/K | |
Specific heat capacity | -100.0 °C | 423 J/(kg·K) Show Material materials with Specific heat capacity of 423 J/(kg·K) |
20.0 °C | 461 J/(kg·K) Show Material materials with Specific heat capacity of 461 J/(kg·K) | |
100.0 °C | 479 J/(kg·K) Show Material materials with Specific heat capacity of 479 J/(kg·K) | |
200.0 °C | 499 J/(kg·K) Show Material materials with Specific heat capacity of 499 J/(kg·K) | |
300.0 °C | 517 J/(kg·K) Show Material materials with Specific heat capacity of 517 J/(kg·K) | |
400.0 °C | 536 J/(kg·K) Show Material materials with Specific heat capacity of 536 J/(kg·K) | |
500.0 °C | 558 J/(kg·K) Show Material materials with Specific heat capacity of 558 J/(kg·K) | |
600.0 °C | 587 J/(kg·K) Show Material materials with Specific heat capacity of 587 J/(kg·K) | |
Thermal conductivity | 20.0 °C | 41.7 W/(m·K) Show Material materials with Thermal conductivity of 41.7 W/(m·K) |
100.0 °C | 43.4 W/(m·K) Show Material materials with Thermal conductivity of 43.4 W/(m·K) | |
200.0 °C | 43.2 W/(m·K) Show Material materials with Thermal conductivity of 43.2 W/(m·K) | |
300.0 °C | 41.4 W/(m·K) Show Material materials with Thermal conductivity of 41.4 W/(m·K) | |
400.0 °C | 39.1 W/(m·K) Show Material materials with Thermal conductivity of 39.1 W/(m·K) | |
500.0 °C | 36.7 W/(m·K) Show Material materials with Thermal conductivity of 36.7 W/(m·K) | |
600.0 °C | 34.1 W/(m·K) Show Material materials with Thermal conductivity of 34.1 W/(m·K) | |
Thermal diffusivity | 20.0 °C | 11.6 mm²/s Show Material materials with Thermal diffusivity of 11.6 mm²/s |
100.0 °C | 11.3 mm²/s Show Material materials with Thermal diffusivity of 11.3 mm²/s | |
200.0 °C | 10.5 mm²/s Show Material materials with Thermal diffusivity of 10.5 mm²/s | |
300.0 °C | 9.5 mm²/s Show Material materials with Thermal diffusivity of 9.5 mm²/s | |
400.0 °C | 8.3 mm²/s Show Material materials with Thermal diffusivity of 8.3 mm²/s | |
500.0 °C | 7.1 mm²/s Show Material materials with Thermal diffusivity of 7.1 mm²/s | |
600.0 °C | 5.8 mm²/s Show Material materials with Thermal diffusivity of 5.8 mm²/s | |
Electrical
Property | Temperature | Value |
---|---|---|
Electrical resistivity | 20.0 °C | 2.5E-7 Ω·m Show Material materials with Electrical resistivity of 2.5E-7 Ω·m |
100.0 °C | 2.95E-7 Ω·m Show Material materials with Electrical resistivity of 2.95E-7 Ω·m | |
200.0 °C | 3.65E-7 Ω·m Show Material materials with Electrical resistivity of 3.65E-7 Ω·m | |
300.0 °C | 4.53E-7 Ω·m Show Material materials with Electrical resistivity of 4.53E-7 Ω·m | |
400.0 °C | 5.56E-7 Ω·m Show Material materials with Electrical resistivity of 5.56E-7 Ω·m | |
500.0 °C | 6.74E-7 Ω·m Show Material materials with Electrical resistivity of 6.74E-7 Ω·m | |
600.0 °C | 8.13E-7 Ω·m Show Material materials with Electrical resistivity of 8.13E-7 Ω·m | |
Chemical properties
Property | Value |
---|---|
Carbon | 0.42 - 0.48 % Show Material materials with Carbon of 0.42 - 0.48 % |
Chromium | 0.4 - 0.6 % Show Material materials with Chromium of 0.4 - 0.6 % |
Copper | 0.3 % Show Material materials with Copper of 0.3 % |
Manganese | 0.5 - 0.8 % Show Material materials with Manganese of 0.5 - 0.8 % |
Phosphorus | 0.03 % Show Material materials with Phosphorus of 0.03 % |
Silicon | 0.4 % Show Material materials with Silicon of 0.4 % |
Sulfur | 0.035 % Show Material materials with Sulfur of 0.035 % |