General
Property | Temperature | Value |
---|---|---|
Density | 20.0 °C | 7.85 g/cm³ Show Material materials with Density of 7.85 g/cm³ |
Mechanical
Property | Temperature | Value | Comment |
---|---|---|---|
Elastic modulus | 20.0 °C | 211 GPa Show Material materials with Elastic modulus of 211 GPa | |
100.0 °C | 204 GPa Show Material materials with Elastic modulus of 204 GPa | ||
200.0 °C | 196 GPa Show Material materials with Elastic modulus of 196 GPa | ||
300.0 °C | 186 GPa Show Material materials with Elastic modulus of 186 GPa | ||
400.0 °C | 177 GPa Show Material materials with Elastic modulus of 177 GPa | ||
450.0 °C | 172 GPa Show Material materials with Elastic modulus of 172 GPa | ||
500.0 °C | 164 GPa Show Material materials with Elastic modulus of 164 GPa | ||
550.0 °C | 152 GPa Show Material materials with Elastic modulus of 152 GPa | ||
600.0 °C | 127 GPa Show Material materials with Elastic modulus of 127 GPa | ||
Elongation | 20.0 °C | 22 % Show Material materials with Elongation of 22 % | |
Poisson's ratio | 23.0 °C | 0.29 [-] Show Material materials with Poisson's ratio of 0.29 [-] | Typical for Medium Carbon Steel |
Reduction of area | 20.0 °C | 45 % Show Material materials with Reduction of area of 45 % | |
Shear modulus | 23.0 °C | 75 - 80 GPa Show Material materials with Shear modulus of 75 - 80 GPa | Typical for Carbon Steel |
Tensile strength | 20.0 °C | 500 - 650 MPa Show Material materials with Tensile strength of 500 - 650 MPa | |
Yield strength Rp0.2 | 20.0 °C | 280 MPa Show Material materials with Yield strength Rp0.2 of 280 MPa | |
200.0 °C | 220 MPa Show Material materials with Yield strength Rp0.2 of 220 MPa | ||
250.0 °C | 203 MPa Show Material materials with Yield strength Rp0.2 of 203 MPa | ||
300.0 °C | 186 MPa Show Material materials with Yield strength Rp0.2 of 186 MPa | ||
350.0 °C | 167 MPa Show Material materials with Yield strength Rp0.2 of 167 MPa | ||
400.0 °C | 147 MPa Show Material materials with Yield strength Rp0.2 of 147 MPa | ||
Thermal
Property | Temperature | Value | Comment |
---|---|---|---|
Coefficient of thermal expansion | 100.0 °C | 1.11E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.11E-5 1/K | |
200.0 °C | 1.21E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.21E-5 1/K | ||
300.0 °C | 1.29E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.29E-5 1/K | ||
400.0 °C | 1.35E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.35E-5 1/K | ||
500.0 °C | 1.39E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.39E-5 1/K | ||
600.0 °C | 1.41E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.41E-5 1/K | ||
Max service temperature | 500 °C Show Material materials with Max service temperature of 500 °C | Typical for Carbon Steel | |
Max service temperature, long | 0 - 350 °C Show Material materials with Max service temperature, long of 0 - 350 °C | ||
Melting point | 1380 - 1514 °C Show Material materials with Melting point of 1380 - 1514 °C | Typical for Medium Carbon Steel | |
Specific heat capacity | 20.0 °C | 460 J/(kg·K) Show Material materials with Specific heat capacity of 460 J/(kg·K) | |
Thermal conductivity | 20.0 °C | 42 W/(m·K) Show Material materials with Thermal conductivity of 42 W/(m·K) |
Electrical
Property | Temperature | Value | Comment |
---|---|---|---|
Electrical resistivity | 23.0 °C | 1.43E-7 - 1.74E-7 Ω·m Show Material materials with Electrical resistivity of 1.43E-7 - 1.74E-7 Ω·m | Typical for Carbon Steel |
Chemical properties
Property | Value |
---|---|
Carbon | 0.32 - 0.39 % Show Material materials with Carbon of 0.32 - 0.39 % |
Manganese | 0.5 - 0.8 % Show Material materials with Manganese of 0.5 - 0.8 % |
Phosphorus | 0.04 % Show Material materials with Phosphorus of 0.04 % |
Silicon | 0.15 - 0.35 % Show Material materials with Silicon of 0.15 - 0.35 % |
Sulfur | 0.035 % Show Material materials with Sulfur of 0.035 % |
Do you have a technical question or need more information about this material?