General
Property | Temperature | Value |
---|---|---|
Density | 20.0 °C | 7.97 - 8.01 g/cm³ Show Material materials with Density of 7.97 - 8.01 g/cm³ |
Mechanical
Property | Temperature | Value |
---|---|---|
Elastic modulus | -100.0 °C | 206 GPa Show Material materials with Elastic modulus of 206 GPa |
20.0 °C | 196 - 197.57 GPa Show Material materials with Elastic modulus of 196 - 197.57 GPa | |
100.0 °C | 190 - 192 GPa Show Material materials with Elastic modulus of 190 - 192 GPa | |
200.0 °C | 182 - 186 GPa Show Material materials with Elastic modulus of 182 - 186 GPa | |
300.0 °C | 174 - 181 GPa Show Material materials with Elastic modulus of 174 - 181 GPa | |
400.0 °C | 166 - 174 GPa Show Material materials with Elastic modulus of 166 - 174 GPa | |
500.0 °C | 158 - 165 GPa Show Material materials with Elastic modulus of 158 - 165 GPa | |
600.0 °C | 150 - 157 GPa Show Material materials with Elastic modulus of 150 - 157 GPa | |
700.0 °C | 142 - 147 GPa Show Material materials with Elastic modulus of 142 - 147 GPa | |
800.0 °C | 134 GPa Show Material materials with Elastic modulus of 134 GPa | |
Elongation | 20.0 °C | 16 % Show Material materials with Elongation of 16 % |
Poisson's ratio | 20.0 °C | 0.28 [-] Show Material materials with Poisson's ratio of 0.28 [-] |
Reduction of area | 20.0 °C | 40 % Show Material materials with Reduction of area of 40 % |
Shear modulus | 20.0 °C | 77.3 GPa Show Material materials with Shear modulus of 77.3 GPa |
Tensile strength | 20.0 °C | 650 - 850 MPa Show Material materials with Tensile strength of 650 - 850 MPa |
Yield strength Rp0.2 | 20.0 °C | 500 MPa Show Material materials with Yield strength Rp0.2 of 500 MPa |
200.0 °C | 432 MPa Show Material materials with Yield strength Rp0.2 of 432 MPa | |
250.0 °C | 412 MPa Show Material materials with Yield strength Rp0.2 of 412 MPa | |
300.0 °C | 393 MPa Show Material materials with Yield strength Rp0.2 of 393 MPa | |
350.0 °C | 372 MPa Show Material materials with Yield strength Rp0.2 of 372 MPa | |
400.0 °C | 353 MPa Show Material materials with Yield strength Rp0.2 of 353 MPa | |
450.0 °C | 334 MPa Show Material materials with Yield strength Rp0.2 of 334 MPa | |
500.0 °C | 314 MPa Show Material materials with Yield strength Rp0.2 of 314 MPa | |
550.0 °C | 284 MPa Show Material materials with Yield strength Rp0.2 of 284 MPa | |
600.0 °C | 255 MPa Show Material materials with Yield strength Rp0.2 of 255 MPa | |
650.0 °C | 206 MPa Show Material materials with Yield strength Rp0.2 of 206 MPa | |
Thermal
Property | Temperature | Value | Comment |
---|---|---|---|
Coefficient of thermal expansion | -100.0 °C | 1.49E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.49E-5 1/K | |
20.0 °C | 1.61E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.61E-5 1/K | ||
100.0 °C | 1.67E-5 - 1.76E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.67E-5 - 1.76E-5 1/K | ||
200.0 °C | 1.72E-5 - 1.77E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.72E-5 - 1.77E-5 1/K | ||
300.0 °C | 1.77E-5 - 1.79E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.77E-5 - 1.79E-5 1/K | ||
400.0 °C | 1.79E-5 - 1.81E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.79E-5 - 1.81E-5 1/K | ||
500.0 °C | 1.79E-5 - 1.84E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.79E-5 - 1.84E-5 1/K | ||
600.0 °C | 1.81E-5 - 1.88E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.81E-5 - 1.88E-5 1/K | ||
700.0 °C | 1.83E-5 - 1.91E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.83E-5 - 1.91E-5 1/K | ||
800.0 °C | 1.86E-5 - 1.94E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.86E-5 - 1.94E-5 1/K | ||
900.0 °C | 1.97E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.97E-5 1/K | ||
1000.0 °C | 2E-5 1/K Show Material materials with Coefficient of thermal expansion of 2E-5 1/K | ||
Max service temperature, long | 0 - 750 °C Show Material materials with Max service temperature, long of 0 - 750 °C | ||
Melting point | 1230 - 1480 °C Show Material materials with Melting point of 1230 - 1480 °C | Typical for Austenitic Stainless Steel | |
Specific heat capacity | -100.0 °C | 440 J/(kg·K) Show Material materials with Specific heat capacity of 440 J/(kg·K) | |
20.0 °C | 460 - 472 J/(kg·K) Show Material materials with Specific heat capacity of 460 - 472 J/(kg·K) | ||
100.0 °C | 487 J/(kg·K) Show Material materials with Specific heat capacity of 487 J/(kg·K) | ||
200.0 °C | 503 J/(kg·K) Show Material materials with Specific heat capacity of 503 J/(kg·K) | ||
300.0 °C | 512 J/(kg·K) Show Material materials with Specific heat capacity of 512 J/(kg·K) | ||
400.0 °C | 520 J/(kg·K) Show Material materials with Specific heat capacity of 520 J/(kg·K) | ||
500.0 °C | 530 J/(kg·K) Show Material materials with Specific heat capacity of 530 J/(kg·K) | ||
600.0 °C | 541 J/(kg·K) Show Material materials with Specific heat capacity of 541 J/(kg·K) | ||
700.0 °C | 551 J/(kg·K) Show Material materials with Specific heat capacity of 551 J/(kg·K) | ||
800.0 °C | 559 J/(kg·K) Show Material materials with Specific heat capacity of 559 J/(kg·K) | ||
900.0 °C | 565 J/(kg·K) Show Material materials with Specific heat capacity of 565 J/(kg·K) | ||
1000.0 °C | 571 J/(kg·K) Show Material materials with Specific heat capacity of 571 J/(kg·K) | ||
Thermal conductivity | 20.0 °C | 13.5 - 15 W/(m·K) Show Material materials with Thermal conductivity of 13.5 - 15 W/(m·K) | |
100.0 °C | 14.9 - 20 W/(m·K) Show Material materials with Thermal conductivity of 14.9 - 20 W/(m·K) | ||
200.0 °C | 16.7 - 20 W/(m·K) Show Material materials with Thermal conductivity of 16.7 - 20 W/(m·K) | ||
300.0 °C | 18.3 - 19 W/(m·K) Show Material materials with Thermal conductivity of 18.3 - 19 W/(m·K) | ||
400.0 °C | 19 - 19.8 W/(m·K) Show Material materials with Thermal conductivity of 19 - 19.8 W/(m·K) | ||
500.0 °C | 21 - 21.3 W/(m·K) Show Material materials with Thermal conductivity of 21 - 21.3 W/(m·K) | ||
600.0 °C | 22 - 22.7 W/(m·K) Show Material materials with Thermal conductivity of 22 - 22.7 W/(m·K) | ||
700.0 °C | 24 - 24.2 W/(m·K) Show Material materials with Thermal conductivity of 24 - 24.2 W/(m·K) | ||
800.0 °C | 25 - 25.6 W/(m·K) Show Material materials with Thermal conductivity of 25 - 25.6 W/(m·K) | ||
Thermal diffusivity | 20.0 °C | 3.6 mm²/s Show Material materials with Thermal diffusivity of 3.6 mm²/s | |
100.0 °C | 3.7 mm²/s Show Material materials with Thermal diffusivity of 3.7 mm²/s | ||
200.0 °C | 4 mm²/s Show Material materials with Thermal diffusivity of 4 mm²/s | ||
300.0 °C | 4.4 mm²/s Show Material materials with Thermal diffusivity of 4.4 mm²/s | ||
400.0 °C | 4.6 mm²/s Show Material materials with Thermal diffusivity of 4.6 mm²/s | ||
500.0 °C | 4.7 mm²/s Show Material materials with Thermal diffusivity of 4.7 mm²/s | ||
600.0 °C | 4.9 mm²/s Show Material materials with Thermal diffusivity of 4.9 mm²/s | ||
700.0 °C | 5.2 mm²/s Show Material materials with Thermal diffusivity of 5.2 mm²/s | ||
800.0 °C | 5.5 mm²/s Show Material materials with Thermal diffusivity of 5.5 mm²/s | ||
Electrical
Property | Temperature | Value |
---|---|---|
Electrical resistivity | 20.0 °C | 7.75E-7 - 8.5E-7 Ω·m Show Material materials with Electrical resistivity of 7.75E-7 - 8.5E-7 Ω·m |
100.0 °C | 8.42E-7 Ω·m Show Material materials with Electrical resistivity of 8.42E-7 Ω·m | |
200.0 °C | 9.04E-7 Ω·m Show Material materials with Electrical resistivity of 9.04E-7 Ω·m | |
300.0 °C | 9.62E-7 Ω·m Show Material materials with Electrical resistivity of 9.62E-7 Ω·m | |
400.0 °C | 1.01E-6 Ω·m Show Material materials with Electrical resistivity of 1.01E-6 Ω·m | |
500.0 °C | 1.06E-6 Ω·m Show Material materials with Electrical resistivity of 1.06E-6 Ω·m | |
600.0 °C | 1.1E-6 Ω·m Show Material materials with Electrical resistivity of 1.1E-6 Ω·m | |
700.0 °C | 1.13E-6 Ω·m Show Material materials with Electrical resistivity of 1.13E-6 Ω·m | |
800.0 °C | 1.16E-6 Ω·m Show Material materials with Electrical resistivity of 1.16E-6 Ω·m | |
Chemical properties
Property | Value |
---|---|
Carbon | 0.04 - 0.1 % Show Material materials with Carbon of 0.04 - 0.1 % |
Chromium | 15.5 - 17.5 % Show Material materials with Chromium of 15.5 - 17.5 % |
Manganese | 1.5 % Show Material materials with Manganese of 1.5 % |
Molybdenum | 1.6 - 2 % Show Material materials with Molybdenum of 1.6 - 2 % |
Nickel | 15.5 - 17.5 % Show Material materials with Nickel of 15.5 - 17.5 % |
Phosphorus | 0.05 % Show Material materials with Phosphorus of 0.05 % |
Silicon | 0.3 - 0.6 % Show Material materials with Silicon of 0.3 - 0.6 % |
Sulfur | 0.03 % Show Material materials with Sulfur of 0.03 % |
Do you have a technical question or need more information about this material?
Post it as a comment below and receive answers from engineers and other community members.