General
Property | Temperature | Value |
---|---|---|
Density | 20.0 °C | 7.84 g/cm³ Show Material materials with Density of 7.84 g/cm³ |
Mechanical
Property | Temperature | Value |
---|---|---|
Elastic modulus | -100.0 °C | 217 GPa Show Material materials with Elastic modulus of 217 GPa |
20.0 °C | 212 - 212.43 GPa Show Material materials with Elastic modulus of 212 - 212.43 GPa | |
100.0 °C | 207 - 209 GPa Show Material materials with Elastic modulus of 207 - 209 GPa | |
200.0 °C | 199 - 202 GPa Show Material materials with Elastic modulus of 199 - 202 GPa | |
300.0 °C | 192 - 195 GPa Show Material materials with Elastic modulus of 192 - 195 GPa | |
400.0 °C | 184 - 187 GPa Show Material materials with Elastic modulus of 184 - 187 GPa | |
500.0 °C | 174.89 - 177 GPa Show Material materials with Elastic modulus of 174.89 - 177 GPa | |
600.0 °C | 163.15 - 167 GPa Show Material materials with Elastic modulus of 163.15 - 167 GPa | |
Elongation | 20.0 °C | 17 - 22 % Show Material materials with Elongation of 17 - 22 % |
Elongation, transverse | 20.0 °C | 18 % Show Material materials with Elongation, transverse of 18 % |
Hardness, Brinell | 20.0 °C | 130 - 175 [-] Show Material materials with Hardness, Brinell of 130 - 175 [-] |
Poisson's ratio | 20.0 °C | 0.28 [-] Show Material materials with Poisson's ratio of 0.28 [-] |
100.0 °C | 0.29 [-] Show Material materials with Poisson's ratio of 0.29 [-] | |
200.0 °C | 0.29 [-] Show Material materials with Poisson's ratio of 0.29 [-] | |
300.0 °C | 0.29 [-] Show Material materials with Poisson's ratio of 0.29 [-] | |
400.0 °C | 0.3 [-] Show Material materials with Poisson's ratio of 0.3 [-] | |
500.0 °C | 0.31 [-] Show Material materials with Poisson's ratio of 0.31 [-] | |
600.0 °C | 0.31 [-] Show Material materials with Poisson's ratio of 0.31 [-] | |
Shear modulus | 20.0 °C | 82.81 GPa Show Material materials with Shear modulus of 82.81 GPa |
100.0 °C | 80.65 GPa Show Material materials with Shear modulus of 80.65 GPa | |
200.0 °C | 77.87 GPa Show Material materials with Shear modulus of 77.87 GPa | |
300.0 °C | 74.93 GPa Show Material materials with Shear modulus of 74.93 GPa | |
400.0 °C | 71.22 GPa Show Material materials with Shear modulus of 71.22 GPa | |
500.0 °C | 66.9 GPa Show Material materials with Shear modulus of 66.9 GPa | |
600.0 °C | 62.11 GPa Show Material materials with Shear modulus of 62.11 GPa | |
Tensile strength | 20.0 °C | 430 - 630 MPa Show Material materials with Tensile strength of 430 - 630 MPa |
200.0 °C | 390 MPa Show Material materials with Tensile strength of 390 MPa | |
250.0 °C | 390 MPa Show Material materials with Tensile strength of 390 MPa | |
300.0 °C | 390 MPa Show Material materials with Tensile strength of 390 MPa | |
350.0 °C | 390 MPa Show Material materials with Tensile strength of 390 MPa | |
400.0 °C | 385 MPa Show Material materials with Tensile strength of 385 MPa | |
450.0 °C | 365 MPa Show Material materials with Tensile strength of 365 MPa | |
500.0 °C | 335 MPa Show Material materials with Tensile strength of 335 MPa | |
Tensile strength, transverse | 20.0 °C | 450 - 600 MPa Show Material materials with Tensile strength, transverse of 450 - 600 MPa |
Yield strength Rp0.2 | 20.0 °C | 240 - 310 MPa Show Material materials with Yield strength Rp0.2 of 240 - 310 MPa |
100.0 °C | 225 - 275 MPa Show Material materials with Yield strength Rp0.2 of 225 - 275 MPa | |
150.0 °C | 215 - 260 MPa Show Material materials with Yield strength Rp0.2 of 215 - 260 MPa | |
200.0 °C | 205 - 245 MPa Show Material materials with Yield strength Rp0.2 of 205 - 245 MPa | |
250.0 °C | 200 - 240 MPa Show Material materials with Yield strength Rp0.2 of 200 - 240 MPa | |
300.0 °C | 190 - 230 MPa Show Material materials with Yield strength Rp0.2 of 190 - 230 MPa | |
350.0 °C | 175 - 215 MPa Show Material materials with Yield strength Rp0.2 of 175 - 215 MPa | |
400.0 °C | 165 - 205 MPa Show Material materials with Yield strength Rp0.2 of 165 - 205 MPa | |
450.0 °C | 155 - 195 MPa Show Material materials with Yield strength Rp0.2 of 155 - 195 MPa | |
500.0 °C | 145 - 185 MPa Show Material materials with Yield strength Rp0.2 of 145 - 185 MPa | |
Yield strength Rp0.2, transverse | 20.0 °C | 260 - 280 MPa Show Material materials with Yield strength Rp0.2, transverse of 260 - 280 MPa |
Thermal
Property | Temperature | Value | Comment |
---|---|---|---|
Coefficient of thermal expansion | -100.0 °C | 1.05E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.05E-5 1/K | |
20.0 °C | 1.15E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.15E-5 1/K | ||
100.0 °C | 1.21E-5 - 1.22E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.21E-5 - 1.22E-5 1/K | ||
200.0 °C | 1.27E-5 - 1.29E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.27E-5 - 1.29E-5 1/K | ||
300.0 °C | 1.32E-5 - 1.34E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.32E-5 - 1.34E-5 1/K | ||
400.0 °C | 1.36E-5 - 1.4E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.36E-5 - 1.4E-5 1/K | ||
500.0 °C | 1.4E-5 - 1.43E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.4E-5 - 1.43E-5 1/K | ||
600.0 °C | 1.44E-5 - 1.46E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.44E-5 - 1.46E-5 1/K | ||
Max service temperature, long | 0 - 530 °C Show Material materials with Max service temperature, long of 0 - 530 °C | ||
Melting point | 1382 - 1529 °C Show Material materials with Melting point of 1382 - 1529 °C | Typical for Chromium Molybdenum Steel | |
Specific heat capacity | -100.0 °C | 423 J/(kg·K) Show Material materials with Specific heat capacity of 423 J/(kg·K) | |
20.0 °C | 461 J/(kg·K) Show Material materials with Specific heat capacity of 461 J/(kg·K) | ||
100.0 °C | 479 - 500 J/(kg·K) Show Material materials with Specific heat capacity of 479 - 500 J/(kg·K) | ||
200.0 °C | 499 - 540 J/(kg·K) Show Material materials with Specific heat capacity of 499 - 540 J/(kg·K) | ||
300.0 °C | 517 - 580 J/(kg·K) Show Material materials with Specific heat capacity of 517 - 580 J/(kg·K) | ||
400.0 °C | 536 - 620 J/(kg·K) Show Material materials with Specific heat capacity of 536 - 620 J/(kg·K) | ||
500.0 °C | 558 - 690 J/(kg·K) Show Material materials with Specific heat capacity of 558 - 690 J/(kg·K) | ||
600.0 °C | 587 - 780 J/(kg·K) Show Material materials with Specific heat capacity of 587 - 780 J/(kg·K) | ||
Thermal conductivity | 20.0 °C | 34.9 W/(m·K) Show Material materials with Thermal conductivity of 34.9 W/(m·K) | |
100.0 °C | 37 - 37.3 W/(m·K) Show Material materials with Thermal conductivity of 37 - 37.3 W/(m·K) | ||
200.0 °C | 38 - 38.2 W/(m·K) Show Material materials with Thermal conductivity of 38 - 38.2 W/(m·K) | ||
300.0 °C | 37.8 - 38 W/(m·K) Show Material materials with Thermal conductivity of 37.8 - 38 W/(m·K) | ||
400.0 °C | 36.6 - 37 W/(m·K) Show Material materials with Thermal conductivity of 36.6 - 37 W/(m·K) | ||
500.0 °C | 35 - 35.2 W/(m·K) Show Material materials with Thermal conductivity of 35 - 35.2 W/(m·K) | ||
600.0 °C | 33 - 33.6 W/(m·K) Show Material materials with Thermal conductivity of 33 - 33.6 W/(m·K) | ||
Thermal diffusivity | 20.0 °C | 9.7 mm²/s Show Material materials with Thermal diffusivity of 9.7 mm²/s | |
100.0 °C | 9.6 mm²/s Show Material materials with Thermal diffusivity of 9.6 mm²/s | ||
200.0 °C | 9.2 mm²/s Show Material materials with Thermal diffusivity of 9.2 mm²/s | ||
300.0 °C | 8.5 mm²/s Show Material materials with Thermal diffusivity of 8.5 mm²/s | ||
400.0 °C | 7.8 mm²/s Show Material materials with Thermal diffusivity of 7.8 mm²/s | ||
500.0 °C | 6.8 mm²/s Show Material materials with Thermal diffusivity of 6.8 mm²/s | ||
600.0 °C | 5.7 mm²/s Show Material materials with Thermal diffusivity of 5.7 mm²/s | ||
Electrical
Property | Temperature | Value |
---|---|---|
Electrical resistivity | 20.0 °C | 2.98E-7 Ω·m Show Material materials with Electrical resistivity of 2.98E-7 Ω·m |
100.0 °C | 3.4E-7 - 3.43E-7 Ω·m Show Material materials with Electrical resistivity of 3.4E-7 - 3.43E-7 Ω·m | |
200.0 °C | 4.1E-7 - 4.13E-7 Ω·m Show Material materials with Electrical resistivity of 4.1E-7 - 4.13E-7 Ω·m | |
300.0 °C | 4.97E-7 - 5E-7 Ω·m Show Material materials with Electrical resistivity of 4.97E-7 - 5E-7 Ω·m | |
400.0 °C | 5.9E-7 - 5.95E-7 Ω·m Show Material materials with Electrical resistivity of 5.9E-7 - 5.95E-7 Ω·m | |
500.0 °C | 7E-7 - 7.03E-7 Ω·m Show Material materials with Electrical resistivity of 7E-7 - 7.03E-7 Ω·m | |
600.0 °C | 8.2E-7 - 8.25E-7 Ω·m Show Material materials with Electrical resistivity of 8.2E-7 - 8.25E-7 Ω·m | |
Chemical properties
Property | Value |
---|---|
Carbon | 0.06 - 0.15 % Show Material materials with Carbon of 0.06 - 0.15 % |
Chromium | 2 - 2.5 % Show Material materials with Chromium of 2 - 2.5 % |
Manganese | 0.4 - 0.7 % Show Material materials with Manganese of 0.4 - 0.7 % |
Molybdenum | 0.9 - 1.2 % Show Material materials with Molybdenum of 0.9 - 1.2 % |
Nickel | 0.5 % Show Material materials with Nickel of 0.5 % |
Phosphorus | 0.04 % Show Material materials with Phosphorus of 0.04 % |
Silicon | 0.4 - 0.5 % Show Material materials with Silicon of 0.4 - 0.5 % |
Sulfur | 0.03 % Show Material materials with Sulfur of 0.03 % |
Do you have a technical question or need more information about this material?