General
Property | Temperature | Value |
---|---|---|
Density | 20.0 °C | 7.85 g/cm³ Show Material materials with Density of 7.85 g/cm³ |
Mechanical
Property | Temperature | Value | Comment |
---|---|---|---|
Elastic modulus | -100.0 °C | 217 GPa Show Material materials with Elastic modulus of 217 GPa | |
20.0 °C | 212 GPa Show Material materials with Elastic modulus of 212 GPa | ||
100.0 °C | 195 - 207 GPa Show Material materials with Elastic modulus of 195 - 207 GPa | ||
200.0 °C | 195 - 199 GPa Show Material materials with Elastic modulus of 195 - 199 GPa | ||
300.0 °C | 185 - 192 GPa Show Material materials with Elastic modulus of 185 - 192 GPa | ||
400.0 °C | 175 - 184 GPa Show Material materials with Elastic modulus of 175 - 184 GPa | ||
500.0 °C | 165 - 175 GPa Show Material materials with Elastic modulus of 165 - 175 GPa | ||
600.0 °C | 155 - 164 GPa Show Material materials with Elastic modulus of 155 - 164 GPa | ||
Elongation | 20.0 °C | 19 - 25 % Show Material materials with Elongation of 19 - 25 % | |
Elongation, transverse | 20.0 °C | 19 - 23 % Show Material materials with Elongation, transverse of 19 - 23 % | |
Poisson's ratio | 23.0 °C | 0.29 [-] Show Material materials with Poisson's ratio of 0.29 [-] | Typical for Low Carbon Steel |
Shear modulus | 23.0 °C | 82 GPa Show Material materials with Shear modulus of 82 GPa | Typical for Low Carbon Steel |
Tensile strength | 20.0 °C | 400 - 540 MPa Show Material materials with Tensile strength of 400 - 540 MPa | |
Tensile strength, transverse | 20.0 °C | 400 - 540 MPa Show Material materials with Tensile strength, transverse of 400 - 540 MPa | |
Yield strength | 20.0 °C | 210 - 250 MPa Show Material materials with Yield strength of 210 - 250 MPa | |
Yield strength Rp0.2 | 20.0 °C | 200 - 250 MPa Show Material materials with Yield strength Rp0.2 of 200 - 250 MPa | |
100.0 °C | 190 - 237 MPa Show Material materials with Yield strength Rp0.2 of 190 - 237 MPa | ||
150.0 °C | 170 - 216 MPa Show Material materials with Yield strength Rp0.2 of 170 - 216 MPa | ||
200.0 °C | 155 - 190 MPa Show Material materials with Yield strength Rp0.2 of 155 - 190 MPa | ||
250.0 °C | 135 - 170 MPa Show Material materials with Yield strength Rp0.2 of 135 - 170 MPa | ||
300.0 °C | 115 - 150 MPa Show Material materials with Yield strength Rp0.2 of 115 - 150 MPa | ||
350.0 °C | 100 - 145 MPa Show Material materials with Yield strength Rp0.2 of 100 - 145 MPa | ||
400.0 °C | 80 - 135 MPa Show Material materials with Yield strength Rp0.2 of 80 - 135 MPa | ||
420.0 °C | 65 - 90 MPa Show Material materials with Yield strength Rp0.2 of 65 - 90 MPa | ||
450.0 °C | 60 - 90 MPa Show Material materials with Yield strength Rp0.2 of 60 - 90 MPa | ||
Thermal
Property | Temperature | Value | Comment |
---|---|---|---|
Coefficient of thermal expansion | -100.0 °C | 1.08E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.08E-5 1/K | |
20.0 °C | 1.19E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.19E-5 1/K | ||
100.0 °C | 1.1E-5 - 1.25E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.1E-5 - 1.25E-5 1/K | ||
200.0 °C | 1.2E-5 - 1.3E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.2E-5 - 1.3E-5 1/K | ||
300.0 °C | 1.3E-5 - 1.36E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.3E-5 - 1.36E-5 1/K | ||
400.0 °C | 1.35E-5 - 1.41E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.35E-5 - 1.41E-5 1/K | ||
500.0 °C | 1.4E-5 - 1.45E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.4E-5 - 1.45E-5 1/K | ||
600.0 °C | 1.4E-5 - 1.49E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.4E-5 - 1.49E-5 1/K | ||
Max service temperature | 500 °C Show Material materials with Max service temperature of 500 °C | Typical for Carbon Steel | |
Melting point | 1480 - 1526 °C Show Material materials with Melting point of 1480 - 1526 °C | Typical for Low Carbon Steel | |
Specific heat capacity | -100.0 °C | 423 J/(kg·K) Show Material materials with Specific heat capacity of 423 J/(kg·K) | |
20.0 °C | 461 J/(kg·K) Show Material materials with Specific heat capacity of 461 J/(kg·K) | ||
100.0 °C | 479 J/(kg·K) Show Material materials with Specific heat capacity of 479 J/(kg·K) | ||
200.0 °C | 499 J/(kg·K) Show Material materials with Specific heat capacity of 499 J/(kg·K) | ||
300.0 °C | 517 J/(kg·K) Show Material materials with Specific heat capacity of 517 J/(kg·K) | ||
400.0 °C | 536 J/(kg·K) Show Material materials with Specific heat capacity of 536 J/(kg·K) | ||
500.0 °C | 558 J/(kg·K) Show Material materials with Specific heat capacity of 558 J/(kg·K) | ||
600.0 °C | 587 J/(kg·K) Show Material materials with Specific heat capacity of 587 J/(kg·K) | ||
Thermal conductivity | 20.0 °C | 51 W/(m·K) Show Material materials with Thermal conductivity of 51 W/(m·K) | |
100.0 °C | 50.8 W/(m·K) Show Material materials with Thermal conductivity of 50.8 W/(m·K) | ||
200.0 °C | 48.7 W/(m·K) Show Material materials with Thermal conductivity of 48.7 W/(m·K) | ||
300.0 °C | 45.8 W/(m·K) Show Material materials with Thermal conductivity of 45.8 W/(m·K) | ||
400.0 °C | 42.5 W/(m·K) Show Material materials with Thermal conductivity of 42.5 W/(m·K) | ||
500.0 °C | 39.2 W/(m·K) Show Material materials with Thermal conductivity of 39.2 W/(m·K) | ||
600.0 °C | 36 W/(m·K) Show Material materials with Thermal conductivity of 36 W/(m·K) | ||
Thermal diffusivity | 20.0 °C | 14.1 mm²/s Show Material materials with Thermal diffusivity of 14.1 mm²/s | |
100.0 °C | 13.1 mm²/s Show Material materials with Thermal diffusivity of 13.1 mm²/s | ||
200.0 °C | 11.7 mm²/s Show Material materials with Thermal diffusivity of 11.7 mm²/s | ||
300.0 °C | 10.4 mm²/s Show Material materials with Thermal diffusivity of 10.4 mm²/s | ||
400.0 °C | 9 mm²/s Show Material materials with Thermal diffusivity of 9 mm²/s | ||
500.0 °C | 7.6 mm²/s Show Material materials with Thermal diffusivity of 7.6 mm²/s | ||
600.0 °C | 6.1 mm²/s Show Material materials with Thermal diffusivity of 6.1 mm²/s | ||
Electrical
Property | Temperature | Value |
---|---|---|
Electrical resistivity | 20.0 °C | 2.04E-7 Ω·m Show Material materials with Electrical resistivity of 2.04E-7 Ω·m |
100.0 °C | 2.52E-7 Ω·m Show Material materials with Electrical resistivity of 2.52E-7 Ω·m | |
200.0 °C | 3.24E-7 Ω·m Show Material materials with Electrical resistivity of 3.24E-7 Ω·m | |
300.0 °C | 4.1E-7 Ω·m Show Material materials with Electrical resistivity of 4.1E-7 Ω·m | |
400.0 °C | 5.12E-7 Ω·m Show Material materials with Electrical resistivity of 5.12E-7 Ω·m | |
500.0 °C | 6.31E-7 Ω·m Show Material materials with Electrical resistivity of 6.31E-7 Ω·m | |
600.0 °C | 7.7E-7 Ω·m Show Material materials with Electrical resistivity of 7.7E-7 Ω·m | |
Magnetic
Property | Value | Comment |
---|---|---|
Curie temperature | 770 °C Show Material materials with Curie temperature of 770 °C | Typical for Low Carbon Steel |
Chemical properties
Property | Value |
---|---|
Aluminium | 0.015 - 0.05 % Show Material materials with Aluminium of 0.015 - 0.05 % |
Carbon | 0.18 - 0.23 % Show Material materials with Carbon of 0.18 - 0.23 % |
Chromium | 0.3 % Show Material materials with Chromium of 0.3 % |
Manganese | 0.4 - 0.9 % Show Material materials with Manganese of 0.4 - 0.9 % |
Phosphorus | 0.03 - 0.04 % Show Material materials with Phosphorus of 0.03 - 0.04 % |
Silicon | 0.15 - 0.4 % Show Material materials with Silicon of 0.15 - 0.4 % |
Sulfur | 0.015 - 0.03 % Show Material materials with Sulfur of 0.015 - 0.03 % |
Do you have a technical question or need more information about this material?
Post it as a comment below and receive answers from engineers and other community members.