DIN 17243 Grade X20CrMoV12-1 quenched and tempered (+QT)

Want to keep this datasheet? Save it now in your required format

Description

High temperature steel for high pressure hydrogenation vessels up to 600 °C. It is scale resistant in air and steam up to 700 °C. Application: in the chemical industry, steam vessel and turbine construction for blades, screws and other high temperature parts

Related Standards

Equivalent Materials

This material data has been provided by WIAM.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValue

Density

20.0 °C

7.76 g/cm³

Show Material materials with Density of 7.76 g/cm³

50.0 °C

7.75 g/cm³

Show Material materials with Density of 7.75 g/cm³

100.0 °C

7.74 g/cm³

Show Material materials with Density of 7.74 g/cm³

150.0 °C

7.73 g/cm³

Show Material materials with Density of 7.73 g/cm³

200.0 °C

7.71 g/cm³

Show Material materials with Density of 7.71 g/cm³

250.0 °C

7.7 g/cm³

Show Material materials with Density of 7.7 g/cm³

300.0 °C

7.68 g/cm³

Show Material materials with Density of 7.68 g/cm³

350.0 °C

7.67 g/cm³

Show Material materials with Density of 7.67 g/cm³

400.0 °C

7.65 g/cm³

Show Material materials with Density of 7.65 g/cm³

450.0 °C

7.64 g/cm³

Show Material materials with Density of 7.64 g/cm³

500.0 °C

7.62 g/cm³

Show Material materials with Density of 7.62 g/cm³

550.0 °C

7.61 g/cm³

Show Material materials with Density of 7.61 g/cm³

600.0 °C

7.59 g/cm³

Show Material materials with Density of 7.59 g/cm³

Mechanical

PropertyTemperatureValue

Elastic modulus

20.0 °C

217.68 - 218 GPa

Show Material materials with Elastic modulus of 217.68 - 218 GPa

50.0 °C

216.02 GPa

Show Material materials with Elastic modulus of 216.02 GPa

100.0 °C

212.98 - 213 GPa

Show Material materials with Elastic modulus of 212.98 - 213 GPa

150.0 °C

209.64 GPa

Show Material materials with Elastic modulus of 209.64 GPa

200.0 °C

206 - 206.21 GPa

Show Material materials with Elastic modulus of 206 - 206.21 GPa

250.0 °C

202.38 GPa

Show Material materials with Elastic modulus of 202.38 GPa

300.0 °C

198 - 198.26 GPa

Show Material materials with Elastic modulus of 198 - 198.26 GPa

350.0 °C

193.94 GPa

Show Material materials with Elastic modulus of 193.94 GPa

400.0 °C

189 - 190 GPa

Show Material materials with Elastic modulus of 189 - 190 GPa

450.0 °C

184.33 GPa

Show Material materials with Elastic modulus of 184.33 GPa

500.0 °C

178.93 - 180 GPa

Show Material materials with Elastic modulus of 178.93 - 180 GPa

550.0 °C

172.85 GPa

Show Material materials with Elastic modulus of 172.85 GPa

600.0 °C

165.79 - 167 GPa

Show Material materials with Elastic modulus of 165.79 - 167 GPa

Unlock all property charts

Elongation

20.0 °C

16 - 17 %

Show Material materials with Elongation of 16 - 17 %

Elongation, transverse

20.0 °C

14 %

Show Material materials with Elongation, transverse of 14 %

Poisson's ratio

20.0 °C

0.28 [-]

Show Material materials with Poisson's ratio of 0.28 [-]

50.0 °C

0.28 [-]

Show Material materials with Poisson's ratio of 0.28 [-]

100.0 °C

0.28 [-]

Show Material materials with Poisson's ratio of 0.28 [-]

150.0 °C

0.28 [-]

Show Material materials with Poisson's ratio of 0.28 [-]

200.0 °C

0.29 [-]

Show Material materials with Poisson's ratio of 0.29 [-]

250.0 °C

0.29 [-]

Show Material materials with Poisson's ratio of 0.29 [-]

300.0 °C

0.29 [-]

Show Material materials with Poisson's ratio of 0.29 [-]

350.0 °C

0.29 [-]

Show Material materials with Poisson's ratio of 0.29 [-]

400.0 °C

0.3 [-]

Show Material materials with Poisson's ratio of 0.3 [-]

450.0 °C

0.3 [-]

Show Material materials with Poisson's ratio of 0.3 [-]

500.0 °C

0.31 [-]

Show Material materials with Poisson's ratio of 0.31 [-]

550.0 °C

0.31 [-]

Show Material materials with Poisson's ratio of 0.31 [-]

600.0 °C

0.31 [-]

Show Material materials with Poisson's ratio of 0.31 [-]

Unlock all property charts

Shear modulus

20.0 °C

84.95 GPa

Show Material materials with Shear modulus of 84.95 GPa

50.0 °C

84.27 GPa

Show Material materials with Shear modulus of 84.27 GPa

100.0 °C

82.99 GPa

Show Material materials with Shear modulus of 82.99 GPa

150.0 °C

81.62 GPa

Show Material materials with Shear modulus of 81.62 GPa

200.0 °C

80.05 GPa

Show Material materials with Shear modulus of 80.05 GPa

250.0 °C

78.48 GPa

Show Material materials with Shear modulus of 78.48 GPa

300.0 °C

76.71 GPa

Show Material materials with Shear modulus of 76.71 GPa

350.0 °C

74.95 GPa

Show Material materials with Shear modulus of 74.95 GPa

400.0 °C

73.08 GPa

Show Material materials with Shear modulus of 73.08 GPa

450.0 °C

70.93 GPa

Show Material materials with Shear modulus of 70.93 GPa

500.0 °C

68.57 GPa

Show Material materials with Shear modulus of 68.57 GPa

550.0 °C

66.02 GPa

Show Material materials with Shear modulus of 66.02 GPa

600.0 °C

63.27 GPa

Show Material materials with Shear modulus of 63.27 GPa

Unlock all property charts

Tensile strength

20.0 °C

690 - 850 MPa

Show Material materials with Tensile strength of 690 - 850 MPa

100.0 °C

650 MPa

Show Material materials with Tensile strength of 650 MPa

150.0 °C

625 MPa

Show Material materials with Tensile strength of 625 MPa

200.0 °C

600 MPa

Show Material materials with Tensile strength of 600 MPa

250.0 °C

590 MPa

Show Material materials with Tensile strength of 590 MPa

300.0 °C

580 MPa

Show Material materials with Tensile strength of 580 MPa

350.0 °C

545 MPa

Show Material materials with Tensile strength of 545 MPa

400.0 °C

510 MPa

Show Material materials with Tensile strength of 510 MPa

450.0 °C

455 MPa

Show Material materials with Tensile strength of 455 MPa

500.0 °C

400 MPa

Show Material materials with Tensile strength of 400 MPa

550.0 °C

325 MPa

Show Material materials with Tensile strength of 325 MPa

Unlock all property charts

Tensile strength, transverse

20.0 °C

690 - 850 MPa

Show Material materials with Tensile strength, transverse of 690 - 850 MPa

Yield strength Rp0.2

20.0 °C

490 - 500 MPa

Show Material materials with Yield strength Rp0.2 of 490 - 500 MPa

100.0 °C

460 MPa

Show Material materials with Yield strength Rp0.2 of 460 MPa

150.0 °C

445 MPa

Show Material materials with Yield strength Rp0.2 of 445 MPa

200.0 °C

430 MPa

Show Material materials with Yield strength Rp0.2 of 430 MPa

250.0 °C

415 MPa

Show Material materials with Yield strength Rp0.2 of 415 MPa

300.0 °C

390 MPa

Show Material materials with Yield strength Rp0.2 of 390 MPa

350.0 °C

380 MPa

Show Material materials with Yield strength Rp0.2 of 380 MPa

400.0 °C

360 MPa

Show Material materials with Yield strength Rp0.2 of 360 MPa

450.0 °C

330 MPa

Show Material materials with Yield strength Rp0.2 of 330 MPa

500.0 °C

290 MPa

Show Material materials with Yield strength Rp0.2 of 290 MPa

550.0 °C

250 MPa

Show Material materials with Yield strength Rp0.2 of 250 MPa

600.0 °C

160 MPa

Show Material materials with Yield strength Rp0.2 of 160 MPa

Unlock all property charts

Yield strength Rp0.2, transverse

20.0 °C

490 - 500 MPa

Show Material materials with Yield strength Rp0.2, transverse of 490 - 500 MPa

Thermal

PropertyTemperatureValueComment

Coefficient of thermal expansion

20.0 °C

1.02E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.02E-5 1/K

100.0 °C

1.05E-5 - 1.08E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.05E-5 - 1.08E-5 1/K

200.0 °C

1.09E-5 - 1.12E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.09E-5 - 1.12E-5 1/K

300.0 °C

1.13E-5 - 1.16E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.13E-5 - 1.16E-5 1/K

400.0 °C

1.16E-5 - 1.19E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.16E-5 - 1.19E-5 1/K

500.0 °C

1.2E-5 - 1.21E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.2E-5 - 1.21E-5 1/K

600.0 °C

1.22E-5 - 1.23E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.22E-5 - 1.23E-5 1/K

Unlock all property charts

Max service temperature, long

0 - 600 °C

Show Material materials with Max service temperature, long of 0 - 600 °C

Melting point

1370 - 1530 °C

Show Material materials with Melting point of 1370 - 1530 °C

Typical for Martensitic Stainless Steel

Specific heat capacity

20.0 °C

439 J/(kg·K)

Show Material materials with Specific heat capacity of 439 J/(kg·K)

100.0 °C

474 - 490 J/(kg·K)

Show Material materials with Specific heat capacity of 474 - 490 J/(kg·K)

200.0 °C

498 - 540 J/(kg·K)

Show Material materials with Specific heat capacity of 498 - 540 J/(kg·K)

300.0 °C

517 - 580 J/(kg·K)

Show Material materials with Specific heat capacity of 517 - 580 J/(kg·K)

400.0 °C

538 - 630 J/(kg·K)

Show Material materials with Specific heat capacity of 538 - 630 J/(kg·K)

500.0 °C

564 - 710 J/(kg·K)

Show Material materials with Specific heat capacity of 564 - 710 J/(kg·K)

600.0 °C

598 - 830 J/(kg·K)

Show Material materials with Specific heat capacity of 598 - 830 J/(kg·K)

Unlock all property charts

Thermal conductivity

20.0 °C

24 W/(m·K)

Show Material materials with Thermal conductivity of 24 W/(m·K)

100.0 °C

24 - 24.4 W/(m·K)

Show Material materials with Thermal conductivity of 24 - 24.4 W/(m·K)

200.0 °C

24.8 - 25 W/(m·K)

Show Material materials with Thermal conductivity of 24.8 - 25 W/(m·K)

300.0 °C

25 - 25.1 W/(m·K)

Show Material materials with Thermal conductivity of 25 - 25.1 W/(m·K)

400.0 °C

25.6 - 26 W/(m·K)

Show Material materials with Thermal conductivity of 25.6 - 26 W/(m·K)

500.0 °C

26 - 26.1 W/(m·K)

Show Material materials with Thermal conductivity of 26 - 26.1 W/(m·K)

600.0 °C

26 - 26.4 W/(m·K)

Show Material materials with Thermal conductivity of 26 - 26.4 W/(m·K)

Unlock all property charts

Thermal diffusivity

20.0 °C

7.1 mm²/s

Show Material materials with Thermal diffusivity of 7.1 mm²/s

100.0 °C

6.3 mm²/s

Show Material materials with Thermal diffusivity of 6.3 mm²/s

200.0 °C

6 mm²/s

Show Material materials with Thermal diffusivity of 6 mm²/s

300.0 °C

5.7 mm²/s

Show Material materials with Thermal diffusivity of 5.7 mm²/s

400.0 °C

5.4 mm²/s

Show Material materials with Thermal diffusivity of 5.4 mm²/s

500.0 °C

4.9 mm²/s

Show Material materials with Thermal diffusivity of 4.9 mm²/s

600.0 °C

4.1 mm²/s

Show Material materials with Thermal diffusivity of 4.1 mm²/s

Unlock all property charts

Electrical

PropertyTemperatureValue

Electrical resistivity

20.0 °C

6.03E-7 Ω·m

Show Material materials with Electrical resistivity of 6.03E-7 Ω·m

50.0 °C

6.26E-7 Ω·m

Show Material materials with Electrical resistivity of 6.26E-7 Ω·m

100.0 °C

6.68E-7 - 6.7E-7 Ω·m

Show Material materials with Electrical resistivity of 6.68E-7 - 6.7E-7 Ω·m

150.0 °C

7.06E-7 Ω·m

Show Material materials with Electrical resistivity of 7.06E-7 Ω·m

200.0 °C

7.4E-7 - 7.43E-7 Ω·m

Show Material materials with Electrical resistivity of 7.4E-7 - 7.43E-7 Ω·m

250.0 °C

7.83E-7 Ω·m

Show Material materials with Electrical resistivity of 7.83E-7 Ω·m

300.0 °C

8.17E-7 - 8.2E-7 Ω·m

Show Material materials with Electrical resistivity of 8.17E-7 - 8.2E-7 Ω·m

350.0 °C

8.54E-7 Ω·m

Show Material materials with Electrical resistivity of 8.54E-7 Ω·m

400.0 °C

8.9E-7 Ω·m

Show Material materials with Electrical resistivity of 8.9E-7 Ω·m

450.0 °C

9.25E-7 Ω·m

Show Material materials with Electrical resistivity of 9.25E-7 Ω·m

500.0 °C

9.6E-7 - 9.62E-7 Ω·m

Show Material materials with Electrical resistivity of 9.6E-7 - 9.62E-7 Ω·m

550.0 °C

9.99E-7 Ω·m

Show Material materials with Electrical resistivity of 9.99E-7 Ω·m

600.0 °C

1.03E-6 - 1.04E-6 Ω·m

Show Material materials with Electrical resistivity of 1.03E-6 - 1.04E-6 Ω·m

Unlock all property charts

Chemical properties

PropertyValue

Carbon

0.17 - 0.23 %

Show Material materials with Carbon of 0.17 - 0.23 %

Chromium

10 - 12.5 %

Show Material materials with Chromium of 10 - 12.5 %

Manganese

1 %

Show Material materials with Manganese of 1 %

Molybdenum

0.8 - 1.2 %

Show Material materials with Molybdenum of 0.8 - 1.2 %

Nickel

0.3 - 0.8 %

Show Material materials with Nickel of 0.3 - 0.8 %

Phosphorus

0.03 %

Show Material materials with Phosphorus of 0.03 %

Silicon

0.5 %

Show Material materials with Silicon of 0.5 %

Sulfur

0.03 %

Show Material materials with Sulfur of 0.03 %

Vanadium

0.25 - 0.35 %

Show Material materials with Vanadium of 0.25 - 0.35 %