GS-X 22 CrMoV 12 1 is usabel upt to 600 °C verwendbar. For valve cases, steam collector cases and turbine housings.

Related Standards

Equivalent Materials

This material data has been provided by WIAM.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValue

Density

20.0 °C

7.7 g/cm³

Show Material materials with Density of 7.7 g/cm³

Mechanical

PropertyTemperatureValueComment

Elastic modulus

20.0 °C

216 GPa

Show Material materials with Elastic modulus of 216 GPa

100.0 °C

209 GPa

Show Material materials with Elastic modulus of 209 GPa

200.0 °C

200 GPa

Show Material materials with Elastic modulus of 200 GPa

300.0 °C

190 GPa

Show Material materials with Elastic modulus of 190 GPa

400.0 °C

179 GPa

Show Material materials with Elastic modulus of 179 GPa

500.0 °C

167 GPa

Show Material materials with Elastic modulus of 167 GPa

600.0 °C

127 GPa

Show Material materials with Elastic modulus of 127 GPa

Poisson's ratio

23.0 °C

0.3 [-]

Show Material materials with Poisson's ratio of 0.3 [-]

Typical for Martensitic Stainless Steel

Shear modulus

23.0 °C

77 GPa

Show Material materials with Shear modulus of 77 GPa

Typical for Martensitic Stainless Steel

Yield strength Rp0.2

550.0 °C

290 MPa

Show Material materials with Yield strength Rp0.2 of 290 MPa

Thermal

PropertyTemperatureValueComment

Coefficient of thermal expansion

100.0 °C

1.05E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.05E-5 1/K

200.0 °C

1.1E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.1E-5 1/K

300.0 °C

1.15E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.15E-5 1/K

400.0 °C

1.19E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.19E-5 1/K

500.0 °C

1.22E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.22E-5 1/K

600.0 °C

1.25E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.25E-5 1/K

Unlock all property charts

Max service temperature, long

300 - 610 °C

Show Material materials with Max service temperature, long of 300 - 610 °C

Melting point

1370 - 1530 °C

Show Material materials with Melting point of 1370 - 1530 °C

Typical for Martensitic Stainless Steel

Specific heat capacity

20.0 °C

460 J/(kg·K)

Show Material materials with Specific heat capacity of 460 J/(kg·K)

Thermal conductivity

20.0 °C

24 W/(m·K)

Show Material materials with Thermal conductivity of 24 W/(m·K)

300.0 °C

25 W/(m·K)

Show Material materials with Thermal conductivity of 25 W/(m·K)

400.0 °C

26 W/(m·K)

Show Material materials with Thermal conductivity of 26 W/(m·K)

500.0 °C

27 W/(m·K)

Show Material materials with Thermal conductivity of 27 W/(m·K)

600.0 °C

27 W/(m·K)

Show Material materials with Thermal conductivity of 27 W/(m·K)

Unlock all property charts

Electrical

PropertyTemperatureValue

Electrical resistivity

20.0 °C

4.5E-7 Ω·m

Show Material materials with Electrical resistivity of 4.5E-7 Ω·m

Chemical properties

PropertyValue

Carbon

0.2 - 0.26 %

Show Material materials with Carbon of 0.2 - 0.26 %

Chromium

11.3 - 12.2 %

Show Material materials with Chromium of 11.3 - 12.2 %

Manganese

0.5 - 0.8 %

Show Material materials with Manganese of 0.5 - 0.8 %

Molybdenum

1 - 1.2 %

Show Material materials with Molybdenum of 1 - 1.2 %

Nickel

0.7 - 1 %

Show Material materials with Nickel of 0.7 - 1 %

Phosphorus

0.03 %

Show Material materials with Phosphorus of 0.03 %

Silicon

0.1 - 0.4 %

Show Material materials with Silicon of 0.1 - 0.4 %

Sulfur

0.02 %

Show Material materials with Sulfur of 0.02 %

Vanadium

0.25 - 0.35 %

Show Material materials with Vanadium of 0.25 - 0.35 %