General
Property | Temperature | Value |
---|---|---|
Density | 20.0 °C | 7.86 g/cm³ Show Material materials with Density of 7.86 g/cm³ |
Mechanical
Property | Temperature | Value | Comment |
---|---|---|---|
Elastic modulus | -100.0 °C | 210 GPa Show Material materials with Elastic modulus of 210 GPa | |
20.0 °C | 204 GPa Show Material materials with Elastic modulus of 204 GPa | ||
100.0 °C | 199 GPa Show Material materials with Elastic modulus of 199 GPa | ||
200.0 °C | 193 GPa Show Material materials with Elastic modulus of 193 GPa | ||
300.0 °C | 186 GPa Show Material materials with Elastic modulus of 186 GPa | ||
400.0 °C | 178 GPa Show Material materials with Elastic modulus of 178 GPa | ||
Elongation | 20.0 °C | 19 % Show Material materials with Elongation of 19 % | |
Poisson's ratio | 23.0 °C | 0.29 [-] Show Material materials with Poisson's ratio of 0.29 [-] | Typical for Nickel Steel |
Shear modulus | 23.0 °C | 76 GPa Show Material materials with Shear modulus of 76 GPa | Typical for Nickel Steel |
Tensile strength | 20.0 °C | 510 - 710 MPa Show Material materials with Tensile strength of 510 - 710 MPa | |
Yield strength | 20.0 °C | 380 - 390 MPa Show Material materials with Yield strength of 380 - 390 MPa |
Thermal
Property | Temperature | Value | Comment |
---|---|---|---|
Coefficient of thermal expansion | -100.0 °C | 1.02E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.02E-5 1/K | |
20.0 °C | 1.12E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.12E-5 1/K | ||
100.0 °C | 1.17E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.17E-5 1/K | ||
200.0 °C | 1.21E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.21E-5 1/K | ||
300.0 °C | 1.25E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.25E-5 1/K | ||
400.0 °C | 1.28E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.28E-5 1/K | ||
Melting point | 1316 - 1595 °C Show Material materials with Melting point of 1316 - 1595 °C | Typical for Nickel Steel | |
Specific heat capacity | -100.0 °C | 440 J/(kg·K) Show Material materials with Specific heat capacity of 440 J/(kg·K) | |
20.0 °C | 463 J/(kg·K) Show Material materials with Specific heat capacity of 463 J/(kg·K) | ||
100.0 °C | 477 J/(kg·K) Show Material materials with Specific heat capacity of 477 J/(kg·K) | ||
200.0 °C | 494 J/(kg·K) Show Material materials with Specific heat capacity of 494 J/(kg·K) | ||
300.0 °C | 510 J/(kg·K) Show Material materials with Specific heat capacity of 510 J/(kg·K) | ||
400.0 °C | 529 J/(kg·K) Show Material materials with Specific heat capacity of 529 J/(kg·K) | ||
Thermal conductivity | -100.0 °C | 29.5 W/(m·K) Show Material materials with Thermal conductivity of 29.5 W/(m·K) | |
20.0 °C | 36.2 W/(m·K) Show Material materials with Thermal conductivity of 36.2 W/(m·K) | ||
100.0 °C | 38.5 W/(m·K) Show Material materials with Thermal conductivity of 38.5 W/(m·K) | ||
200.0 °C | 39 W/(m·K) Show Material materials with Thermal conductivity of 39 W/(m·K) | ||
300.0 °C | 38.3 W/(m·K) Show Material materials with Thermal conductivity of 38.3 W/(m·K) | ||
400.0 °C | 36.2 W/(m·K) Show Material materials with Thermal conductivity of 36.2 W/(m·K) | ||
Thermal diffusivity | 20.0 °C | 10 mm²/s Show Material materials with Thermal diffusivity of 10 mm²/s | |
100.0 °C | 10 mm²/s Show Material materials with Thermal diffusivity of 10 mm²/s | ||
200.0 °C | 9.6 mm²/s Show Material materials with Thermal diffusivity of 9.6 mm²/s | ||
300.0 °C | 8.8 mm²/s Show Material materials with Thermal diffusivity of 8.8 mm²/s | ||
400.0 °C | 7.7 mm²/s Show Material materials with Thermal diffusivity of 7.7 mm²/s | ||
Electrical
Property | Temperature | Value |
---|---|---|
Electrical resistivity | -100.0 °C | 1.95E-7 Ω·m Show Material materials with Electrical resistivity of 1.95E-7 Ω·m |
20.0 °C | 2.61E-7 Ω·m Show Material materials with Electrical resistivity of 2.61E-7 Ω·m | |
100.0 °C | 3.1E-7 Ω·m Show Material materials with Electrical resistivity of 3.1E-7 Ω·m | |
200.0 °C | 3.78E-7 Ω·m Show Material materials with Electrical resistivity of 3.78E-7 Ω·m | |
300.0 °C | 4.57E-7 Ω·m Show Material materials with Electrical resistivity of 4.57E-7 Ω·m | |
400.0 °C | 5.57E-7 Ω·m Show Material materials with Electrical resistivity of 5.57E-7 Ω·m | |
Chemical properties
Property | Value |
---|---|
Carbon | 0.15 % Show Material materials with Carbon of 0.15 % |
Manganese | 0.3 - 0.8 % Show Material materials with Manganese of 0.3 - 0.8 % |
Nickel | 4.5 - 5.3 % Show Material materials with Nickel of 4.5 - 5.3 % |
Phosphorus | 0.03 % Show Material materials with Phosphorus of 0.03 % |
Silicon | 0.35 % Show Material materials with Silicon of 0.35 % |
Sulfur | 0.02 % Show Material materials with Sulfur of 0.02 % |
Vanadium | 0.05 % Show Material materials with Vanadium of 0.05 % |