General
Property | Temperature | Value |
---|---|---|
Density | 20.0 °C | 7.92 g/cm³ Show Material materials with Density of 7.92 g/cm³ |
Mechanical
Property | Temperature | Value |
---|---|---|
Elastic modulus | -100.0 °C | 206 GPa Show Material materials with Elastic modulus of 206 GPa |
20.0 °C | 196 - 198.1 GPa Show Material materials with Elastic modulus of 196 - 198.1 GPa | |
100.0 °C | 190 - 194 GPa Show Material materials with Elastic modulus of 190 - 194 GPa | |
200.0 °C | 182 - 186 GPa Show Material materials with Elastic modulus of 182 - 186 GPa | |
300.0 °C | 174 - 179 GPa Show Material materials with Elastic modulus of 174 - 179 GPa | |
400.0 °C | 166 - 172 GPa Show Material materials with Elastic modulus of 166 - 172 GPa | |
500.0 °C | 158 - 165 GPa Show Material materials with Elastic modulus of 158 - 165 GPa | |
600.0 °C | 150 GPa Show Material materials with Elastic modulus of 150 GPa | |
700.0 °C | 142 GPa Show Material materials with Elastic modulus of 142 GPa | |
800.0 °C | 134 GPa Show Material materials with Elastic modulus of 134 GPa | |
Elongation | 20.0 °C | 50 % Show Material materials with Elongation of 50 % |
Poisson's ratio | 20.0 °C | 0.29 [-] Show Material materials with Poisson's ratio of 0.29 [-] |
Reduction of area | 20.0 °C | 55 % Show Material materials with Reduction of area of 55 % |
Shear modulus | 20.0 °C | 75.7 GPa Show Material materials with Shear modulus of 75.7 GPa |
Tensile strength | 20.0 °C | 460 - 680 MPa Show Material materials with Tensile strength of 460 - 680 MPa |
Yield strength | 20.0 °C | 180 MPa Show Material materials with Yield strength of 180 MPa |
Yield strength Rp0.2 | 50.0 °C | 162 MPa Show Material materials with Yield strength Rp0.2 of 162 MPa |
100.0 °C | 147 MPa Show Material materials with Yield strength Rp0.2 of 147 MPa | |
150.0 °C | 132 MPa Show Material materials with Yield strength Rp0.2 of 132 MPa | |
200.0 °C | 118 MPa Show Material materials with Yield strength Rp0.2 of 118 MPa | |
250.0 °C | 108 MPa Show Material materials with Yield strength Rp0.2 of 108 MPa | |
300.0 °C | 100 MPa Show Material materials with Yield strength Rp0.2 of 100 MPa | |
Yield strength Rp1.0 | 50.0 °C | 201 MPa Show Material materials with Yield strength Rp1.0 of 201 MPa |
100.0 °C | 181 MPa Show Material materials with Yield strength Rp1.0 of 181 MPa | |
150.0 °C | 162 MPa Show Material materials with Yield strength Rp1.0 of 162 MPa | |
200.0 °C | 147 MPa Show Material materials with Yield strength Rp1.0 of 147 MPa | |
250.0 °C | 137 MPa Show Material materials with Yield strength Rp1.0 of 137 MPa | |
300.0 °C | 127 MPa Show Material materials with Yield strength Rp1.0 of 127 MPa | |
Thermal
Property | Temperature | Value | Comment |
---|---|---|---|
Coefficient of thermal expansion | -100.0 °C | 1.49E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.49E-5 1/K | |
20.0 °C | 1.61E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.61E-5 1/K | ||
100.0 °C | 1.6E-5 - 1.67E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.6E-5 - 1.67E-5 1/K | ||
200.0 °C | 1.7E-5 - 1.72E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.7E-5 - 1.72E-5 1/K | ||
300.0 °C | 1.7E-5 - 1.77E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.7E-5 - 1.77E-5 1/K | ||
400.0 °C | 1.8E-5 - 1.81E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.8E-5 - 1.81E-5 1/K | ||
500.0 °C | 1.8E-5 - 1.84E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.8E-5 - 1.84E-5 1/K | ||
600.0 °C | 1.88E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.88E-5 1/K | ||
700.0 °C | 1.91E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.91E-5 1/K | ||
800.0 °C | 1.94E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.94E-5 1/K | ||
Max service temperature, long | 0 - 400 °C Show Material materials with Max service temperature, long of 0 - 400 °C | ||
Melting point | 1230 - 1480 °C Show Material materials with Melting point of 1230 - 1480 °C | Typical for Austenitic Stainless Steel | |
Specific heat capacity | -100.0 °C | 440 J/(kg·K) Show Material materials with Specific heat capacity of 440 J/(kg·K) | |
20.0 °C | 472 J/(kg·K) Show Material materials with Specific heat capacity of 472 J/(kg·K) | ||
100.0 °C | 487 J/(kg·K) Show Material materials with Specific heat capacity of 487 J/(kg·K) | ||
200.0 °C | 503 J/(kg·K) Show Material materials with Specific heat capacity of 503 J/(kg·K) | ||
300.0 °C | 512 J/(kg·K) Show Material materials with Specific heat capacity of 512 J/(kg·K) | ||
400.0 °C | 520 J/(kg·K) Show Material materials with Specific heat capacity of 520 J/(kg·K) | ||
500.0 °C | 530 J/(kg·K) Show Material materials with Specific heat capacity of 530 J/(kg·K) | ||
600.0 °C | 541 J/(kg·K) Show Material materials with Specific heat capacity of 541 J/(kg·K) | ||
700.0 °C | 551 J/(kg·K) Show Material materials with Specific heat capacity of 551 J/(kg·K) | ||
800.0 °C | 559 J/(kg·K) Show Material materials with Specific heat capacity of 559 J/(kg·K) | ||
Thermal conductivity | 20.0 °C | 13.9 W/(m·K) Show Material materials with Thermal conductivity of 13.9 W/(m·K) | |
100.0 °C | 15.4 W/(m·K) Show Material materials with Thermal conductivity of 15.4 W/(m·K) | ||
200.0 °C | 17.2 W/(m·K) Show Material materials with Thermal conductivity of 17.2 W/(m·K) | ||
300.0 °C | 18.7 W/(m·K) Show Material materials with Thermal conductivity of 18.7 W/(m·K) | ||
400.0 °C | 20.2 W/(m·K) Show Material materials with Thermal conductivity of 20.2 W/(m·K) | ||
500.0 °C | 21.6 W/(m·K) Show Material materials with Thermal conductivity of 21.6 W/(m·K) | ||
600.0 °C | 23 W/(m·K) Show Material materials with Thermal conductivity of 23 W/(m·K) | ||
700.0 °C | 24.4 W/(m·K) Show Material materials with Thermal conductivity of 24.4 W/(m·K) | ||
800.0 °C | 25.8 W/(m·K) Show Material materials with Thermal conductivity of 25.8 W/(m·K) | ||
Thermal diffusivity | 20.0 °C | 3.7 mm²/s Show Material materials with Thermal diffusivity of 3.7 mm²/s | |
100.0 °C | 3.9 mm²/s Show Material materials with Thermal diffusivity of 3.9 mm²/s | ||
200.0 °C | 4.2 mm²/s Show Material materials with Thermal diffusivity of 4.2 mm²/s | ||
300.0 °C | 4.5 mm²/s Show Material materials with Thermal diffusivity of 4.5 mm²/s | ||
400.0 °C | 4.7 mm²/s Show Material materials with Thermal diffusivity of 4.7 mm²/s | ||
500.0 °C | 4.8 mm²/s Show Material materials with Thermal diffusivity of 4.8 mm²/s | ||
600.0 °C | 5 mm²/s Show Material materials with Thermal diffusivity of 5 mm²/s | ||
700.0 °C | 5.3 mm²/s Show Material materials with Thermal diffusivity of 5.3 mm²/s | ||
800.0 °C | 5.6 mm²/s Show Material materials with Thermal diffusivity of 5.6 mm²/s | ||
Electrical
Property | Temperature | Value |
---|---|---|
Electrical resistivity | 20.0 °C | 7.35E-7 Ω·m Show Material materials with Electrical resistivity of 7.35E-7 Ω·m |
100.0 °C | 8E-7 Ω·m Show Material materials with Electrical resistivity of 8E-7 Ω·m | |
200.0 °C | 8.68E-7 Ω·m Show Material materials with Electrical resistivity of 8.68E-7 Ω·m | |
300.0 °C | 9.33E-7 Ω·m Show Material materials with Electrical resistivity of 9.33E-7 Ω·m | |
400.0 °C | 9.89E-7 Ω·m Show Material materials with Electrical resistivity of 9.89E-7 Ω·m | |
500.0 °C | 1.04E-6 Ω·m Show Material materials with Electrical resistivity of 1.04E-6 Ω·m | |
600.0 °C | 1.08E-6 Ω·m Show Material materials with Electrical resistivity of 1.08E-6 Ω·m | |
700.0 °C | 1.12E-6 Ω·m Show Material materials with Electrical resistivity of 1.12E-6 Ω·m | |
800.0 °C | 1.15E-6 Ω·m Show Material materials with Electrical resistivity of 1.15E-6 Ω·m | |
Chemical properties
Property | Value |
---|---|
Carbon | 0.03 % Show Material materials with Carbon of 0.03 % |
Chromium | 18 - 20 % Show Material materials with Chromium of 18 - 20 % |
Manganese | 2 % Show Material materials with Manganese of 2 % |
Nickel | 10 - 12.5 % Show Material materials with Nickel of 10 - 12.5 % |
Phosphorus | 0.05 % Show Material materials with Phosphorus of 0.05 % |
Silicon | 1 % Show Material materials with Silicon of 1 % |
Sulfur | 0.03 % Show Material materials with Sulfur of 0.03 % |