General
Property | Temperature | Value |
---|---|---|
Density | 20.0 °C | 7.88 g/cm³ Show Material materials with Density of 7.88 g/cm³ |
Mechanical
Property | Temperature | Value | Comment |
---|---|---|---|
Elastic modulus | 23.0 °C | 195 GPa Show Material materials with Elastic modulus of 195 GPa | Typical for Austenitic Stainless Steel |
Elongation | 20.0 °C | 30 % Show Material materials with Elongation of 30 % | |
Poisson's ratio | 23.0 °C | 0.3 [-] Show Material materials with Poisson's ratio of 0.3 [-] | Typical for Austenitic Stainless Steel |
Shear modulus | 23.0 °C | 77 GPa Show Material materials with Shear modulus of 77 GPa | Typical for Austenitic Stainless Steel |
Tensile strength | 20.0 °C | 440 - 640 MPa Show Material materials with Tensile strength of 440 - 640 MPa | |
Yield strength Rp1.0 | 20.0 °C | 200 MPa Show Material materials with Yield strength Rp1.0 of 200 MPa | |
100.0 °C | 160 MPa Show Material materials with Yield strength Rp1.0 of 160 MPa | ||
200.0 °C | 125 MPa Show Material materials with Yield strength Rp1.0 of 125 MPa | ||
300.0 °C | 110 MPa Show Material materials with Yield strength Rp1.0 of 110 MPa | ||
Thermal
Property | Temperature | Value | Comment |
---|---|---|---|
Coefficient of thermal expansion | 100.0 °C | 1.68E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.68E-5 1/K | |
300.0 °C | 1.79E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.79E-5 1/K | ||
500.0 °C | 1.86E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.86E-5 1/K | ||
Max service temperature, long | -196 - 550 °C Show Material materials with Max service temperature, long of -196 - 550 °C | ||
Melting point | 1230 - 1480 °C Show Material materials with Melting point of 1230 - 1480 °C | Typical for Austenitic Stainless Steel | |
Specific heat capacity | 20.0 °C | 530 J/(kg·K) Show Material materials with Specific heat capacity of 530 J/(kg·K) | |
Thermal conductivity | 50.0 °C | 15.2 W/(m·K) Show Material materials with Thermal conductivity of 15.2 W/(m·K) | |
100.0 °C | 16.5 W/(m·K) Show Material materials with Thermal conductivity of 16.5 W/(m·K) | ||
Electrical
Property | Temperature | Value | Comment |
---|---|---|---|
Electrical resistivity | 23.0 °C | 8.5E-7 Ω·m Show Material materials with Electrical resistivity of 8.5E-7 Ω·m | Typical for Austenitic Stainless Steel |
Chemical properties
Property | Value |
---|---|
Carbon | 0.07 % Show Material materials with Carbon of 0.07 % |
Chromium | 18 - 20 % Show Material materials with Chromium of 18 - 20 % |
Manganese | 1.5 % Show Material materials with Manganese of 1.5 % |
Nickel | 8 - 11 % Show Material materials with Nickel of 8 - 11 % |
Phosphorus | 0.04 % Show Material materials with Phosphorus of 0.04 % |
Silicon | 1.5 % Show Material materials with Silicon of 1.5 % |
Sulfur | 0.03 % Show Material materials with Sulfur of 0.03 % |
Do you have a technical question or need more information about this material?