General
Property | Temperature | Value |
---|---|---|
Density | 20.0 °C | 7.84 g/cm³ Show Material materials with Density of 7.84 g/cm³ |
Mechanical
Property | Temperature | Value | Comment |
---|---|---|---|
Elastic modulus | 20.0 °C | 210 GPa Show Material materials with Elastic modulus of 210 GPa | |
Elongation | 20.0 °C | 14 % Show Material materials with Elongation of 14 % | |
Elongation, transverse | 20.0 °C | 16 % Show Material materials with Elongation, transverse of 16 % | |
Poisson's ratio | 23.0 °C | 0.3 [-] Show Material materials with Poisson's ratio of 0.3 [-] | Typical for Steel |
Tensile strength | 20.0 °C | 760 - 900 MPa Show Material materials with Tensile strength of 760 - 900 MPa | |
Tensile strength, transverse | 20.0 °C | 760 - 900 MPa Show Material materials with Tensile strength, transverse of 760 - 900 MPa | |
Yield strength | 20.0 °C | 690 MPa Show Material materials with Yield strength of 690 MPa | |
Yield strength, transverse | 20.0 °C | 690 MPa Show Material materials with Yield strength, transverse of 690 MPa |
Thermal
Property | Temperature | Value |
---|---|---|
Coefficient of thermal expansion | 100.0 °C | 1.2E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.2E-5 1/K |
Max service temperature, long | -50 - 0 °C Show Material materials with Max service temperature, long of -50 - 0 °C | |
Specific heat capacity | 20.0 °C | 430 J/(kg·K) Show Material materials with Specific heat capacity of 430 J/(kg·K) |
Thermal conductivity | 20.0 °C | 38 W/(m·K) Show Material materials with Thermal conductivity of 38 W/(m·K) |
Electrical
Property | Temperature | Value |
---|---|---|
Electrical resistivity | 20.0 °C | 2.8E-7 Ω·m Show Material materials with Electrical resistivity of 2.8E-7 Ω·m |
Chemical properties
Property | Value |
---|---|
Boron | 5E-4 % Show Material materials with Boron of 5E-4 % |
Carbon | 0.12 - 0.2 % Show Material materials with Carbon of 0.12 - 0.2 % |
Chromium | 0.4 - 0.65 % Show Material materials with Chromium of 0.4 - 0.65 % |
Manganese | 0.7 - 1 % Show Material materials with Manganese of 0.7 - 1 % |
Molybdenum | 0.15 - 0.25 % Show Material materials with Molybdenum of 0.15 - 0.25 % |
Phosphorus | 0.03 % Show Material materials with Phosphorus of 0.03 % |
Silicon | 0.2 - 0.35 % Show Material materials with Silicon of 0.2 - 0.35 % |
Sulfur | 0.015 % Show Material materials with Sulfur of 0.015 % |
Titanium | 0.05 % Show Material materials with Titanium of 0.05 % |
Vanadium | 0.03 - 0.08 % Show Material materials with Vanadium of 0.03 - 0.08 % |