General
Property | Temperature | Value |
---|---|---|
Density | 20.0 °C | 7.58 - 7.7 g/cm³ Show Material materials with Density of 7.58 - 7.7 g/cm³ |
Mechanical
Property | Temperature | Value | Comment |
---|---|---|---|
Elastic modulus | 20.0 °C | 218 - 220 GPa Show Material materials with Elastic modulus of 218 - 220 GPa | |
100.0 °C | 213 - 216 GPa Show Material materials with Elastic modulus of 213 - 216 GPa | ||
200.0 °C | 206 - 209 GPa Show Material materials with Elastic modulus of 206 - 209 GPa | ||
300.0 °C | 198 - 200 GPa Show Material materials with Elastic modulus of 198 - 200 GPa | ||
400.0 °C | 190 - 192 GPa Show Material materials with Elastic modulus of 190 - 192 GPa | ||
500.0 °C | 180 - 183 GPa Show Material materials with Elastic modulus of 180 - 183 GPa | ||
600.0 °C | 167 GPa Show Material materials with Elastic modulus of 167 GPa | ||
700.0 °C | 150 GPa Show Material materials with Elastic modulus of 150 GPa | ||
Hardness, Brinell | 20.0 °C | 260 [-] Show Material materials with Hardness, Brinell of 260 [-] | |
Poisson's ratio | 23.0 °C | 0.3 [-] Show Material materials with Poisson's ratio of 0.3 [-] | Typical for Martensitic Stainless Steel |
Shear modulus | 23.0 °C | 77 GPa Show Material materials with Shear modulus of 77 GPa | Typical for Martensitic Stainless Steel |
Tensile strength | 20.0 °C | 830 MPa Show Material materials with Tensile strength of 830 MPa |
Thermal
Property | Temperature | Value | Comment |
---|---|---|---|
Coefficient of thermal expansion | 20.0 °C | 1.02E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.02E-5 1/K | |
100.0 °C | 1.04E-5 - 1.05E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.04E-5 - 1.05E-5 1/K | ||
200.0 °C | 1.08E-5 - 1.09E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.08E-5 - 1.09E-5 1/K | ||
300.0 °C | 1.12E-5 - 1.13E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.12E-5 - 1.13E-5 1/K | ||
400.0 °C | 1.16E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.16E-5 1/K | ||
500.0 °C | 1.19E-5 - 1.2E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.19E-5 - 1.2E-5 1/K | ||
600.0 °C | 1.22E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.22E-5 1/K | ||
700.0 °C | 1.24E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.24E-5 1/K | ||
Melting point | 1370 - 1530 °C Show Material materials with Melting point of 1370 - 1530 °C | Typical for Martensitic Stainless Steel | |
Specific heat capacity | 20.0 °C | 430 - 439 J/(kg·K) Show Material materials with Specific heat capacity of 430 - 439 J/(kg·K) | |
100.0 °C | 474 J/(kg·K) Show Material materials with Specific heat capacity of 474 J/(kg·K) | ||
200.0 °C | 492 J/(kg·K) Show Material materials with Specific heat capacity of 492 J/(kg·K) | ||
300.0 °C | 517 J/(kg·K) Show Material materials with Specific heat capacity of 517 J/(kg·K) | ||
400.0 °C | 538 J/(kg·K) Show Material materials with Specific heat capacity of 538 J/(kg·K) | ||
500.0 °C | 564 J/(kg·K) Show Material materials with Specific heat capacity of 564 J/(kg·K) | ||
600.0 °C | 598 J/(kg·K) Show Material materials with Specific heat capacity of 598 J/(kg·K) | ||
700.0 °C | 647 J/(kg·K) Show Material materials with Specific heat capacity of 647 J/(kg·K) | ||
Thermal conductivity | 20.0 °C | 15 - 15.7 W/(m·K) Show Material materials with Thermal conductivity of 15 - 15.7 W/(m·K) | |
100.0 °C | 17.1 W/(m·K) Show Material materials with Thermal conductivity of 17.1 W/(m·K) | ||
200.0 °C | 18.6 W/(m·K) Show Material materials with Thermal conductivity of 18.6 W/(m·K) | ||
300.0 °C | 20 W/(m·K) Show Material materials with Thermal conductivity of 20 W/(m·K) | ||
400.0 °C | 21.2 W/(m·K) Show Material materials with Thermal conductivity of 21.2 W/(m·K) | ||
500.0 °C | 22.3 W/(m·K) Show Material materials with Thermal conductivity of 22.3 W/(m·K) | ||
600.0 °C | 23.1 W/(m·K) Show Material materials with Thermal conductivity of 23.1 W/(m·K) | ||
700.0 °C | 23.8 W/(m·K) Show Material materials with Thermal conductivity of 23.8 W/(m·K) | ||
Thermal diffusivity | 20.0 °C | 4.7 mm²/s Show Material materials with Thermal diffusivity of 4.7 mm²/s | |
100.0 °C | 4.5 mm²/s Show Material materials with Thermal diffusivity of 4.5 mm²/s | ||
200.0 °C | 4.6 mm²/s Show Material materials with Thermal diffusivity of 4.6 mm²/s | ||
300.0 °C | 4.7 mm²/s Show Material materials with Thermal diffusivity of 4.7 mm²/s | ||
400.0 °C | 4.5 mm²/s Show Material materials with Thermal diffusivity of 4.5 mm²/s | ||
500.0 °C | 4.3 mm²/s Show Material materials with Thermal diffusivity of 4.3 mm²/s | ||
600.0 °C | 3.7 mm²/s Show Material materials with Thermal diffusivity of 3.7 mm²/s | ||
700.0 °C | 3 mm²/s Show Material materials with Thermal diffusivity of 3 mm²/s | ||
Electrical
Property | Temperature | Value |
---|---|---|
Electrical resistivity | 20.0 °C | 8E-7 - 9.19E-7 Ω·m Show Material materials with Electrical resistivity of 8E-7 - 9.19E-7 Ω·m |
100.0 °C | 9.48E-7 Ω·m Show Material materials with Electrical resistivity of 9.48E-7 Ω·m | |
200.0 °C | 9.87E-7 Ω·m Show Material materials with Electrical resistivity of 9.87E-7 Ω·m | |
300.0 °C | 1.03E-6 Ω·m Show Material materials with Electrical resistivity of 1.03E-6 Ω·m | |
400.0 °C | 1.07E-6 Ω·m Show Material materials with Electrical resistivity of 1.07E-6 Ω·m | |
500.0 °C | 1.12E-6 Ω·m Show Material materials with Electrical resistivity of 1.12E-6 Ω·m | |
600.0 °C | 1.18E-6 Ω·m Show Material materials with Electrical resistivity of 1.18E-6 Ω·m | |
700.0 °C | 1.24E-6 Ω·m Show Material materials with Electrical resistivity of 1.24E-6 Ω·m | |
Chemical properties
Property | Value |
---|---|
Carbon | 0.48 - 0.6 % Show Material materials with Carbon of 0.48 - 0.6 % |
Chromium | 13 - 15 % Show Material materials with Chromium of 13 - 15 % |
Manganese | 1 % Show Material materials with Manganese of 1 % |
Molybdenum | 0.5 - 0.8 % Show Material materials with Molybdenum of 0.5 - 0.8 % |
Phosphorus | 0.04 % Show Material materials with Phosphorus of 0.04 % |
Silicon | 1 % Show Material materials with Silicon of 1 % |
Sulfur | 0.015 % Show Material materials with Sulfur of 0.015 % |
Vanadium | 0.15 % Show Material materials with Vanadium of 0.15 % |