General
Property | Temperature | Value |
---|---|---|
Density | 20.0 °C | 7.7 - 7.73 g/cm³ Show Material materials with Density of 7.7 - 7.73 g/cm³ |
Mechanical
Property | Temperature | Value |
---|---|---|
Elastic modulus | 20.0 °C | 217 - 220 GPa Show Material materials with Elastic modulus of 217 - 220 GPa |
100.0 °C | 215 - 216 GPa Show Material materials with Elastic modulus of 215 - 216 GPa | |
200.0 °C | 188 - 209 GPa Show Material materials with Elastic modulus of 188 - 209 GPa | |
300.0 °C | 164 - 200 GPa Show Material materials with Elastic modulus of 164 - 200 GPa | |
400.0 °C | 192 GPa Show Material materials with Elastic modulus of 192 GPa | |
500.0 °C | 183 GPa Show Material materials with Elastic modulus of 183 GPa | |
Elongation | 20.0 °C | 24 % Show Material materials with Elongation of 24 % |
Hardness, Brinell | 20.0 °C | 180 [-] Show Material materials with Hardness, Brinell of 180 [-] |
Poisson's ratio | 20.0 °C | 0.29 [-] Show Material materials with Poisson's ratio of 0.29 [-] |
Shear modulus | 20.0 °C | 84.82 GPa Show Material materials with Shear modulus of 84.82 GPa |
Tensile strength | 20.0 °C | 380 - 530 MPa Show Material materials with Tensile strength of 380 - 530 MPa |
Yield strength Rp0.2 | 20.0 °C | 220 MPa Show Material materials with Yield strength Rp0.2 of 220 MPa |
50.0 °C | 215 MPa Show Material materials with Yield strength Rp0.2 of 215 MPa | |
100.0 °C | 195 MPa Show Material materials with Yield strength Rp0.2 of 195 MPa | |
150.0 °C | 180 MPa Show Material materials with Yield strength Rp0.2 of 180 MPa | |
200.0 °C | 170 MPa Show Material materials with Yield strength Rp0.2 of 170 MPa | |
250.0 °C | 160 MPa Show Material materials with Yield strength Rp0.2 of 160 MPa | |
300.0 °C | 155 MPa Show Material materials with Yield strength Rp0.2 of 155 MPa | |
Thermal
Property | Temperature | Value | Comment |
---|---|---|---|
Coefficient of thermal expansion | 20.0 °C | 1.02E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.02E-5 1/K | |
100.0 °C | 1.04E-5 - 1.05E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.04E-5 - 1.05E-5 1/K | ||
200.0 °C | 1.08E-5 - 1.09E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.08E-5 - 1.09E-5 1/K | ||
300.0 °C | 1.12E-5 - 1.13E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.12E-5 - 1.13E-5 1/K | ||
400.0 °C | 1.16E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.16E-5 1/K | ||
500.0 °C | 1.19E-5 - 1.2E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.19E-5 - 1.2E-5 1/K | ||
600.0 °C | 1.22E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.22E-5 1/K | ||
Melting point | 1425 - 1530 °C Show Material materials with Melting point of 1425 - 1530 °C | Typical for Ferritic Stainless Steel | |
Specific heat capacity | 20.0 °C | 430 - 439 J/(kg·K) Show Material materials with Specific heat capacity of 430 - 439 J/(kg·K) | |
100.0 °C | 474 J/(kg·K) Show Material materials with Specific heat capacity of 474 J/(kg·K) | ||
200.0 °C | 498 J/(kg·K) Show Material materials with Specific heat capacity of 498 J/(kg·K) | ||
300.0 °C | 517 J/(kg·K) Show Material materials with Specific heat capacity of 517 J/(kg·K) | ||
400.0 °C | 538 J/(kg·K) Show Material materials with Specific heat capacity of 538 J/(kg·K) | ||
500.0 °C | 564 J/(kg·K) Show Material materials with Specific heat capacity of 564 J/(kg·K) | ||
600.0 °C | 598 J/(kg·K) Show Material materials with Specific heat capacity of 598 J/(kg·K) | ||
Thermal conductivity | 20.0 °C | 20 - 25.9 W/(m·K) Show Material materials with Thermal conductivity of 20 - 25.9 W/(m·K) | |
100.0 °C | 25.3 W/(m·K) Show Material materials with Thermal conductivity of 25.3 W/(m·K) | ||
200.0 °C | 25.2 W/(m·K) Show Material materials with Thermal conductivity of 25.2 W/(m·K) | ||
300.0 °C | 25.2 W/(m·K) Show Material materials with Thermal conductivity of 25.2 W/(m·K) | ||
400.0 °C | 25.4 W/(m·K) Show Material materials with Thermal conductivity of 25.4 W/(m·K) | ||
500.0 °C | 25.7 W/(m·K) Show Material materials with Thermal conductivity of 25.7 W/(m·K) | ||
600.0 °C | 25.9 W/(m·K) Show Material materials with Thermal conductivity of 25.9 W/(m·K) | ||
Thermal diffusivity | 20.0 °C | 7.6 mm²/s Show Material materials with Thermal diffusivity of 7.6 mm²/s | |
100.0 °C | 6.6 mm²/s Show Material materials with Thermal diffusivity of 6.6 mm²/s | ||
200.0 °C | 6.1 mm²/s Show Material materials with Thermal diffusivity of 6.1 mm²/s | ||
300.0 °C | 5.8 mm²/s Show Material materials with Thermal diffusivity of 5.8 mm²/s | ||
400.0 °C | 5.3 mm²/s Show Material materials with Thermal diffusivity of 5.3 mm²/s | ||
500.0 °C | 4.8 mm²/s Show Material materials with Thermal diffusivity of 4.8 mm²/s | ||
600.0 °C | 4.1 mm²/s Show Material materials with Thermal diffusivity of 4.1 mm²/s | ||
Electrical
Property | Temperature | Value |
---|---|---|
Electrical resistivity | 20.0 °C | 5.59E-7 - 7E-7 Ω·m Show Material materials with Electrical resistivity of 5.59E-7 - 7E-7 Ω·m |
100.0 °C | 6.4E-7 Ω·m Show Material materials with Electrical resistivity of 6.4E-7 Ω·m | |
200.0 °C | 7.32E-7 Ω·m Show Material materials with Electrical resistivity of 7.32E-7 Ω·m | |
300.0 °C | 8.17E-7 Ω·m Show Material materials with Electrical resistivity of 8.17E-7 Ω·m | |
400.0 °C | 8.97E-7 Ω·m Show Material materials with Electrical resistivity of 8.97E-7 Ω·m | |
500.0 °C | 9.74E-7 Ω·m Show Material materials with Electrical resistivity of 9.74E-7 Ω·m | |
600.0 °C | 1.05E-6 Ω·m Show Material materials with Electrical resistivity of 1.05E-6 Ω·m | |
Chemical properties
Property | Value |
---|---|
Carbon | 0.015 % Show Material materials with Carbon of 0.015 % |
Chromium | 14 - 16 % Show Material materials with Chromium of 14 - 16 % |
Manganese | 0.5 % Show Material materials with Manganese of 0.5 % |
Nitrogen | 0.02 % Show Material materials with Nitrogen of 0.02 % |
Phosphorus | 0.03 % Show Material materials with Phosphorus of 0.03 % |
Silicon | 0.5 % Show Material materials with Silicon of 0.5 % |
Sulfur | 0.02 % Show Material materials with Sulfur of 0.02 % |
Titanium | 0.25 - 0.4 % Show Material materials with Titanium of 0.25 - 0.4 % |