General
Property | Temperature | Value |
---|---|---|
Density | 20.0 °C | 7.7 - 7.76 g/cm³ Show Material materials with Density of 7.7 - 7.76 g/cm³ |
Mechanical
Property | Temperature | Value |
---|---|---|
Elastic modulus | 20.0 °C | 217.68 - 218 GPa Show Material materials with Elastic modulus of 217.68 - 218 GPa |
100.0 °C | 213 GPa Show Material materials with Elastic modulus of 213 GPa | |
200.0 °C | 206 GPa Show Material materials with Elastic modulus of 206 GPa | |
300.0 °C | 198 GPa Show Material materials with Elastic modulus of 198 GPa | |
400.0 °C | 189 - 190 GPa Show Material materials with Elastic modulus of 189 - 190 GPa | |
500.0 °C | 179 - 180 GPa Show Material materials with Elastic modulus of 179 - 180 GPa | |
600.0 °C | 166 - 167 GPa Show Material materials with Elastic modulus of 166 - 167 GPa | |
Elongation, transverse | 20.0 °C | 11 % Show Material materials with Elongation, transverse of 11 % |
Poisson's ratio | 20.0 °C | 0.28 [-] Show Material materials with Poisson's ratio of 0.28 [-] |
Reduction of area, transverse | 20.0 °C | 40 % Show Material materials with Reduction of area, transverse of 40 % |
Shear modulus | 20.0 °C | 84.95 GPa Show Material materials with Shear modulus of 84.95 GPa |
Tensile strength, transverse | 20.0 °C | 750 - 900 MPa Show Material materials with Tensile strength, transverse of 750 - 900 MPa |
Yield strength Rp0.2 | 100.0 °C | 575 MPa Show Material materials with Yield strength Rp0.2 of 575 MPa |
200.0 °C | 530 MPa Show Material materials with Yield strength Rp0.2 of 530 MPa | |
250.0 °C | 505 MPa Show Material materials with Yield strength Rp0.2 of 505 MPa | |
300.0 °C | 480 MPa Show Material materials with Yield strength Rp0.2 of 480 MPa | |
350.0 °C | 450 MPa Show Material materials with Yield strength Rp0.2 of 450 MPa | |
400.0 °C | 425 MPa Show Material materials with Yield strength Rp0.2 of 425 MPa | |
450.0 °C | 380 MPa Show Material materials with Yield strength Rp0.2 of 380 MPa | |
500.0 °C | 345 MPa Show Material materials with Yield strength Rp0.2 of 345 MPa | |
550.0 °C | 285 MPa Show Material materials with Yield strength Rp0.2 of 285 MPa | |
600.0 °C | 205 MPa Show Material materials with Yield strength Rp0.2 of 205 MPa | |
Yield strength Rp0.2, transverse | 20.0 °C | 600 MPa Show Material materials with Yield strength Rp0.2, transverse of 600 MPa |
Thermal
Property | Temperature | Value | Comment |
---|---|---|---|
Coefficient of thermal expansion | 20.0 °C | 1.02E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.02E-5 1/K | |
100.0 °C | 1.05E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.05E-5 1/K | ||
200.0 °C | 1.09E-5 - 1.1E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.09E-5 - 1.1E-5 1/K | ||
300.0 °C | 1.13E-5 - 1.15E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.13E-5 - 1.15E-5 1/K | ||
400.0 °C | 1.16E-5 - 1.2E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.16E-5 - 1.2E-5 1/K | ||
500.0 °C | 1.2E-5 - 1.23E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.2E-5 - 1.23E-5 1/K | ||
600.0 °C | 1.22E-5 - 1.25E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.22E-5 - 1.25E-5 1/K | ||
Max service temperature, long | 0 - 600 °C Show Material materials with Max service temperature, long of 0 - 600 °C | ||
Melting point | 1370 - 1530 °C Show Material materials with Melting point of 1370 - 1530 °C | Typical for Martensitic Stainless Steel | |
Specific heat capacity | 20.0 °C | 439 J/(kg·K) Show Material materials with Specific heat capacity of 439 J/(kg·K) | |
100.0 °C | 474 J/(kg·K) Show Material materials with Specific heat capacity of 474 J/(kg·K) | ||
200.0 °C | 498 J/(kg·K) Show Material materials with Specific heat capacity of 498 J/(kg·K) | ||
300.0 °C | 517 J/(kg·K) Show Material materials with Specific heat capacity of 517 J/(kg·K) | ||
400.0 °C | 538 J/(kg·K) Show Material materials with Specific heat capacity of 538 J/(kg·K) | ||
500.0 °C | 564 J/(kg·K) Show Material materials with Specific heat capacity of 564 J/(kg·K) | ||
600.0 °C | 598 J/(kg·K) Show Material materials with Specific heat capacity of 598 J/(kg·K) | ||
Thermal conductivity | 20.0 °C | 24 W/(m·K) Show Material materials with Thermal conductivity of 24 W/(m·K) | |
100.0 °C | 24 - 24.4 W/(m·K) Show Material materials with Thermal conductivity of 24 - 24.4 W/(m·K) | ||
200.0 °C | 24.8 - 25 W/(m·K) Show Material materials with Thermal conductivity of 24.8 - 25 W/(m·K) | ||
300.0 °C | 25 - 25.1 W/(m·K) Show Material materials with Thermal conductivity of 25 - 25.1 W/(m·K) | ||
400.0 °C | 25.6 - 26 W/(m·K) Show Material materials with Thermal conductivity of 25.6 - 26 W/(m·K) | ||
500.0 °C | 26 - 26.1 W/(m·K) Show Material materials with Thermal conductivity of 26 - 26.1 W/(m·K) | ||
600.0 °C | 26 - 26.4 W/(m·K) Show Material materials with Thermal conductivity of 26 - 26.4 W/(m·K) | ||
Thermal diffusivity | 20.0 °C | 7.1 mm²/s Show Material materials with Thermal diffusivity of 7.1 mm²/s | |
100.0 °C | 6.3 mm²/s Show Material materials with Thermal diffusivity of 6.3 mm²/s | ||
200.0 °C | 6 mm²/s Show Material materials with Thermal diffusivity of 6 mm²/s | ||
300.0 °C | 5.7 mm²/s Show Material materials with Thermal diffusivity of 5.7 mm²/s | ||
400.0 °C | 5.4 mm²/s Show Material materials with Thermal diffusivity of 5.4 mm²/s | ||
500.0 °C | 4.9 mm²/s Show Material materials with Thermal diffusivity of 4.9 mm²/s | ||
600.0 °C | 4.1 mm²/s Show Material materials with Thermal diffusivity of 4.1 mm²/s | ||
Electrical
Property | Temperature | Value |
---|---|---|
Electrical resistivity | 20.0 °C | 6.03E-7 Ω·m Show Material materials with Electrical resistivity of 6.03E-7 Ω·m |
100.0 °C | 6.68E-7 Ω·m Show Material materials with Electrical resistivity of 6.68E-7 Ω·m | |
200.0 °C | 7.43E-7 Ω·m Show Material materials with Electrical resistivity of 7.43E-7 Ω·m | |
300.0 °C | 8.17E-7 Ω·m Show Material materials with Electrical resistivity of 8.17E-7 Ω·m | |
400.0 °C | 8.9E-7 Ω·m Show Material materials with Electrical resistivity of 8.9E-7 Ω·m | |
500.0 °C | 9.62E-7 Ω·m Show Material materials with Electrical resistivity of 9.62E-7 Ω·m | |
600.0 °C | 1.04E-6 Ω·m Show Material materials with Electrical resistivity of 1.04E-6 Ω·m | |
Chemical properties
Property | Value |
---|---|
Carbon | 0.2 - 0.26 % Show Material materials with Carbon of 0.2 - 0.26 % |
Chromium | 11 - 12.5 % Show Material materials with Chromium of 11 - 12.5 % |
Manganese | 0.3 - 0.8 % Show Material materials with Manganese of 0.3 - 0.8 % |
Molybdenum | 0.8 - 1.2 % Show Material materials with Molybdenum of 0.8 - 1.2 % |
Nickel | 0.3 - 0.8 % Show Material materials with Nickel of 0.3 - 0.8 % |
Phosphorus | 0.02 - 0.03 % Show Material materials with Phosphorus of 0.02 - 0.03 % |
Silicon | 0.2 - 0.5 % Show Material materials with Silicon of 0.2 - 0.5 % |
Sulfur | 0.007 - 0.02 % Show Material materials with Sulfur of 0.007 - 0.02 % |
Vanadium | 0.25 - 0.35 % Show Material materials with Vanadium of 0.25 - 0.35 % |