General
Property | Temperature | Value |
---|---|---|
Density | 20.0 °C | 7.85 g/cm³ Show Material materials with Density of 7.85 g/cm³ |
Mechanical
Property | Temperature | Value | Comment |
---|---|---|---|
Elastic modulus | -100.0 °C | 217 GPa Show Material materials with Elastic modulus of 217 GPa | |
20.0 °C | 212 GPa Show Material materials with Elastic modulus of 212 GPa | ||
100.0 °C | 207 GPa Show Material materials with Elastic modulus of 207 GPa | ||
200.0 °C | 199 - 200 GPa Show Material materials with Elastic modulus of 199 - 200 GPa | ||
300.0 °C | 192 - 193 GPa Show Material materials with Elastic modulus of 192 - 193 GPa | ||
400.0 °C | 184 GPa Show Material materials with Elastic modulus of 184 GPa | ||
500.0 °C | 175 GPa Show Material materials with Elastic modulus of 175 GPa | ||
600.0 °C | 164 GPa Show Material materials with Elastic modulus of 164 GPa | ||
Poisson's ratio | 23.0 °C | 0.3 [-] Show Material materials with Poisson's ratio of 0.3 [-] | Typical for Steel |
Yield strength Rp0.2 | 200.0 °C | 500 MPa Show Material materials with Yield strength Rp0.2 of 500 MPa | |
250.0 °C | 480 MPa Show Material materials with Yield strength Rp0.2 of 480 MPa | ||
300.0 °C | 465 MPa Show Material materials with Yield strength Rp0.2 of 465 MPa | ||
350.0 °C | 445 MPa Show Material materials with Yield strength Rp0.2 of 445 MPa | ||
400.0 °C | 425 MPa Show Material materials with Yield strength Rp0.2 of 425 MPa | ||
450.0 °C | 400 MPa Show Material materials with Yield strength Rp0.2 of 400 MPa | ||
500.0 °C | 365 MPa Show Material materials with Yield strength Rp0.2 of 365 MPa | ||
Thermal
Property | Temperature | Value |
---|---|---|
Coefficient of thermal expansion | -100.0 °C | 1.05E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.05E-5 1/K |
20.0 °C | 1.15E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.15E-5 1/K | |
100.0 °C | 1.11E-5 - 1.21E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.11E-5 - 1.21E-5 1/K | |
200.0 °C | 1.21E-5 - 1.27E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.21E-5 - 1.27E-5 1/K | |
300.0 °C | 1.29E-5 - 1.32E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.29E-5 - 1.32E-5 1/K | |
400.0 °C | 1.35E-5 - 1.36E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.35E-5 - 1.36E-5 1/K | |
500.0 °C | 1.39E-5 - 1.4E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.39E-5 - 1.4E-5 1/K | |
600.0 °C | 1.41E-5 - 1.44E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.41E-5 - 1.44E-5 1/K | |
Specific heat capacity | -100.0 °C | 423 J/(kg·K) Show Material materials with Specific heat capacity of 423 J/(kg·K) |
20.0 °C | 461 J/(kg·K) Show Material materials with Specific heat capacity of 461 J/(kg·K) | |
100.0 °C | 479 J/(kg·K) Show Material materials with Specific heat capacity of 479 J/(kg·K) | |
200.0 °C | 499 J/(kg·K) Show Material materials with Specific heat capacity of 499 J/(kg·K) | |
300.0 °C | 517 J/(kg·K) Show Material materials with Specific heat capacity of 517 J/(kg·K) | |
400.0 °C | 536 J/(kg·K) Show Material materials with Specific heat capacity of 536 J/(kg·K) | |
500.0 °C | 558 J/(kg·K) Show Material materials with Specific heat capacity of 558 J/(kg·K) | |
600.0 °C | 587 J/(kg·K) Show Material materials with Specific heat capacity of 587 J/(kg·K) | |
Thermal conductivity | 20.0 °C | 47.1 W/(m·K) Show Material materials with Thermal conductivity of 47.1 W/(m·K) |
100.0 °C | 46 - 47.1 W/(m·K) Show Material materials with Thermal conductivity of 46 - 47.1 W/(m·K) | |
200.0 °C | 45.9 - 46 W/(m·K) Show Material materials with Thermal conductivity of 45.9 - 46 W/(m·K) | |
300.0 °C | 43.8 - 46 W/(m·K) Show Material materials with Thermal conductivity of 43.8 - 46 W/(m·K) | |
400.0 °C | 41.3 - 44 W/(m·K) Show Material materials with Thermal conductivity of 41.3 - 44 W/(m·K) | |
500.0 °C | 38.7 - 43 W/(m·K) Show Material materials with Thermal conductivity of 38.7 - 43 W/(m·K) | |
600.0 °C | 36 - 41 W/(m·K) Show Material materials with Thermal conductivity of 36 - 41 W/(m·K) | |
Thermal diffusivity | 20.0 °C | 13 mm²/s Show Material materials with Thermal diffusivity of 13 mm²/s |
100.0 °C | 12.1 mm²/s Show Material materials with Thermal diffusivity of 12.1 mm²/s | |
200.0 °C | 11.1 mm²/s Show Material materials with Thermal diffusivity of 11.1 mm²/s | |
300.0 °C | 9.9 mm²/s Show Material materials with Thermal diffusivity of 9.9 mm²/s | |
400.0 °C | 8.7 mm²/s Show Material materials with Thermal diffusivity of 8.7 mm²/s | |
500.0 °C | 7.4 mm²/s Show Material materials with Thermal diffusivity of 7.4 mm²/s | |
600.0 °C | 6 mm²/s Show Material materials with Thermal diffusivity of 6 mm²/s | |
Electrical
Property | Temperature | Value |
---|---|---|
Electrical resistivity | 20.0 °C | 2.21E-7 Ω·m Show Material materials with Electrical resistivity of 2.21E-7 Ω·m |
100.0 °C | 2.72E-7 Ω·m Show Material materials with Electrical resistivity of 2.72E-7 Ω·m | |
200.0 °C | 3.44E-7 Ω·m Show Material materials with Electrical resistivity of 3.44E-7 Ω·m | |
300.0 °C | 4.28E-7 Ω·m Show Material materials with Electrical resistivity of 4.28E-7 Ω·m | |
400.0 °C | 5.26E-7 Ω·m Show Material materials with Electrical resistivity of 5.26E-7 Ω·m | |
500.0 °C | 6.39E-7 Ω·m Show Material materials with Electrical resistivity of 6.39E-7 Ω·m | |
600.0 °C | 7.7E-7 Ω·m Show Material materials with Electrical resistivity of 7.7E-7 Ω·m | |
Chemical properties
Property | Value |
---|---|
Carbon | 0.17 - 0.25 % Show Material materials with Carbon of 0.17 - 0.25 % |
Chromium | 1.1 - 1.4 % Show Material materials with Chromium of 1.1 - 1.4 % |
Manganese | 0.3 - 0.8 % Show Material materials with Manganese of 0.3 - 0.8 % |
Molybdenum | 0.8 - 1 % Show Material materials with Molybdenum of 0.8 - 1 % |
Nickel | 0.5 - 0.75 % Show Material materials with Nickel of 0.5 - 0.75 % |
Phosphorus | 0.02 % Show Material materials with Phosphorus of 0.02 % |
Silicon | 0.3 % Show Material materials with Silicon of 0.3 % |
Sulfur | 0.018 % Show Material materials with Sulfur of 0.018 % |
Vanadium | 0.25 - 0.35 % Show Material materials with Vanadium of 0.25 - 0.35 % |