General
Property | Temperature | Value |
---|---|---|
Density | 20.0 °C | 7.8 - 7.85 g/cm³ Show Material materials with Density of 7.8 - 7.85 g/cm³ |
Mechanical
Property | Temperature | Value | Comment |
---|---|---|---|
Elastic modulus | -100.0 °C | 217 GPa Show Material materials with Elastic modulus of 217 GPa | |
20.0 °C | 212 GPa Show Material materials with Elastic modulus of 212 GPa | ||
100.0 °C | 207 GPa Show Material materials with Elastic modulus of 207 GPa | ||
200.0 °C | 199 GPa Show Material materials with Elastic modulus of 199 GPa | ||
300.0 °C | 192 GPa Show Material materials with Elastic modulus of 192 GPa | ||
400.0 °C | 184 GPa Show Material materials with Elastic modulus of 184 GPa | ||
500.0 °C | 175 GPa Show Material materials with Elastic modulus of 175 GPa | ||
600.0 °C | 164 GPa Show Material materials with Elastic modulus of 164 GPa | ||
Elongation, transverse | 20.0 °C | 11 - 13 % Show Material materials with Elongation, transverse of 11 - 13 % | |
Poisson's ratio | 23.0 °C | 0.3 [-] Show Material materials with Poisson's ratio of 0.3 [-] | Typical for Steel |
Reduction of area, transverse | 20.0 °C | 40 % Show Material materials with Reduction of area, transverse of 40 % | |
Tensile strength, transverse | 20.0 °C | 750 - 1050 MPa Show Material materials with Tensile strength, transverse of 750 - 1050 MPa | |
Yield strength Rp0.2 | 100.0 °C | 570 - 710 MPa Show Material materials with Yield strength Rp0.2 of 570 - 710 MPa | |
200.0 °C | 545 - 675 MPa Show Material materials with Yield strength Rp0.2 of 545 - 675 MPa | ||
250.0 °C | 530 - 650 MPa Show Material materials with Yield strength Rp0.2 of 530 - 650 MPa | ||
300.0 °C | 510 - 630 MPa Show Material materials with Yield strength Rp0.2 of 510 - 630 MPa | ||
350.0 °C | 485 - 600 MPa Show Material materials with Yield strength Rp0.2 of 485 - 600 MPa | ||
400.0 °C | 450 - 555 MPa Show Material materials with Yield strength Rp0.2 of 450 - 555 MPa | ||
450.0 °C | 400 - 505 MPa Show Material materials with Yield strength Rp0.2 of 400 - 505 MPa | ||
500.0 °C | 340 - 445 MPa Show Material materials with Yield strength Rp0.2 of 340 - 445 MPa | ||
Yield strength Rp0.2, transverse | 20.0 °C | 600 - 750 MPa Show Material materials with Yield strength Rp0.2, transverse of 600 - 750 MPa |
Thermal
Property | Temperature | Value |
---|---|---|
Coefficient of thermal expansion | -100.0 °C | 1.05E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.05E-5 1/K |
20.0 °C | 1.15E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.15E-5 1/K | |
100.0 °C | 1.21E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.21E-5 1/K | |
200.0 °C | 1.27E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.27E-5 1/K | |
300.0 °C | 1.32E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.32E-5 1/K | |
400.0 °C | 1.36E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.36E-5 1/K | |
500.0 °C | 1.4E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.4E-5 1/K | |
600.0 °C | 1.44E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.44E-5 1/K | |
Specific heat capacity | -100.0 °C | 423 J/(kg·K) Show Material materials with Specific heat capacity of 423 J/(kg·K) |
20.0 °C | 461 J/(kg·K) Show Material materials with Specific heat capacity of 461 J/(kg·K) | |
100.0 °C | 479 J/(kg·K) Show Material materials with Specific heat capacity of 479 J/(kg·K) | |
200.0 °C | 499 J/(kg·K) Show Material materials with Specific heat capacity of 499 J/(kg·K) | |
300.0 °C | 517 J/(kg·K) Show Material materials with Specific heat capacity of 517 J/(kg·K) | |
400.0 °C | 536 J/(kg·K) Show Material materials with Specific heat capacity of 536 J/(kg·K) | |
500.0 °C | 558 J/(kg·K) Show Material materials with Specific heat capacity of 558 J/(kg·K) | |
600.0 °C | 587 J/(kg·K) Show Material materials with Specific heat capacity of 587 J/(kg·K) | |
Thermal conductivity | 20.0 °C | 33.7 W/(m·K) Show Material materials with Thermal conductivity of 33.7 W/(m·K) |
100.0 °C | 36.2 W/(m·K) Show Material materials with Thermal conductivity of 36.2 W/(m·K) | |
200.0 °C | 37.8 W/(m·K) Show Material materials with Thermal conductivity of 37.8 W/(m·K) | |
300.0 °C | 37.2 W/(m·K) Show Material materials with Thermal conductivity of 37.2 W/(m·K) | |
400.0 °C | 35.7 W/(m·K) Show Material materials with Thermal conductivity of 35.7 W/(m·K) | |
500.0 °C | 34 W/(m·K) Show Material materials with Thermal conductivity of 34 W/(m·K) | |
600.0 °C | 32 W/(m·K) Show Material materials with Thermal conductivity of 32 W/(m·K) | |
Thermal diffusivity | 20.0 °C | 9.4 mm²/s Show Material materials with Thermal diffusivity of 9.4 mm²/s |
100.0 °C | 9.4 mm²/s Show Material materials with Thermal diffusivity of 9.4 mm²/s | |
200.0 °C | 9.2 mm²/s Show Material materials with Thermal diffusivity of 9.2 mm²/s | |
300.0 °C | 8.5 mm²/s Show Material materials with Thermal diffusivity of 8.5 mm²/s | |
400.0 °C | 7.6 mm²/s Show Material materials with Thermal diffusivity of 7.6 mm²/s | |
500.0 °C | 6.6 mm²/s Show Material materials with Thermal diffusivity of 6.6 mm²/s | |
600.0 °C | 5.4 mm²/s Show Material materials with Thermal diffusivity of 5.4 mm²/s | |
Electrical
Property | Temperature | Value |
---|---|---|
Electrical resistivity | 20.0 °C | 3.09E-7 Ω·m Show Material materials with Electrical resistivity of 3.09E-7 Ω·m |
100.0 °C | 3.54E-7 Ω·m Show Material materials with Electrical resistivity of 3.54E-7 Ω·m | |
200.0 °C | 4.18E-7 Ω·m Show Material materials with Electrical resistivity of 4.18E-7 Ω·m | |
300.0 °C | 5.05E-7 Ω·m Show Material materials with Electrical resistivity of 5.05E-7 Ω·m | |
400.0 °C | 6.09E-7 Ω·m Show Material materials with Electrical resistivity of 6.09E-7 Ω·m | |
500.0 °C | 7.27E-7 Ω·m Show Material materials with Electrical resistivity of 7.27E-7 Ω·m | |
600.0 °C | 8.67E-7 Ω·m Show Material materials with Electrical resistivity of 8.67E-7 Ω·m | |
Chemical properties
Property | Value |
---|---|
Carbon | 0.22 - 0.32 % Show Material materials with Carbon of 0.22 - 0.32 % |
Chromium | 1.2 - 1.8 % Show Material materials with Chromium of 1.2 - 1.8 % |
Manganese | 0.15 - 0.4 % Show Material materials with Manganese of 0.15 - 0.4 % |
Molybdenum | 0.25 - 0.45 % Show Material materials with Molybdenum of 0.25 - 0.45 % |
Nickel | 2.4 - 3.1 % Show Material materials with Nickel of 2.4 - 3.1 % |
Phosphorus | 0.01 % Show Material materials with Phosphorus of 0.01 % |
Silicon | 0.15 % Show Material materials with Silicon of 0.15 % |
Sulfur | 7E-3 % Show Material materials with Sulfur of 7E-3 % |
Vanadium | 0.05 - 0.15 % Show Material materials with Vanadium of 0.05 - 0.15 % |