General
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Density | 20 °C | 7.85 g/cm³ Show Material materials with Density of 7.85 g/cm³ | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire |
Mechanical
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Elastic modulus | -100 °C | 217 GPa Show Material materials with Elastic modulus of 217 GPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | |
20 °C | 212 GPa Show Material materials with Elastic modulus of 212 GPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
100 °C | 207 GPa Show Material materials with Elastic modulus of 207 GPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
200 °C | 199 GPa Show Material materials with Elastic modulus of 199 GPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
300 °C | 192 GPa Show Material materials with Elastic modulus of 192 GPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
400 °C | 184 GPa Show Material materials with Elastic modulus of 184 GPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
500 °C | 175 GPa Show Material materials with Elastic modulus of 175 GPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
600 °C | 164 GPa Show Material materials with Elastic modulus of 164 GPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
Elongation | 17.9 % Show Material materials with Elongation of 17.9 % | Predicted Value, A200 | ||||
22.9 % Show Material materials with Elongation of 22.9 % | Predicted Value, A5 | |||||
37.6 % Show Material materials with Elongation of 37.6 % | Predicted Value, A50 | |||||
20 °C | 8 % Show Material materials with Elongation of 8 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | A80 Transverse | |
20 °C | 9 % Show Material materials with Elongation of 9 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | A80 Transverse | |
20 °C | 10 % Show Material materials with Elongation of 10 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | A80 Transverse | |
20 °C | 10 % Show Material materials with Elongation of 10 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | A80 | |
20 °C | 11 % Show Material materials with Elongation of 11 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | A80 Transverse | |
20 °C | 11 % Show Material materials with Elongation of 11 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | A80 | |
20 °C | 12 % Show Material materials with Elongation of 12 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | A80 Transverse | |
20 °C | 12 % Show Material materials with Elongation of 12 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | A80 | |
20 °C | 13 % Show Material materials with Elongation of 13 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | A80 | |
20 °C | 13 % Show Material materials with Elongation of 13 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | Transverse | |
20 °C | 14 % Show Material materials with Elongation of 14 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | A80 | |
20 °C | 14 % Show Material materials with Elongation of 14 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | Transverse | |
20 °C | 15 % Show Material materials with Elongation of 15 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | Transverse | |
20 °C | 15 % Show Material materials with Elongation of 15 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 16 % Show Material materials with Elongation of 16 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | Transverse | |
20 °C | 16 % Show Material materials with Elongation of 16 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 17 % Show Material materials with Elongation of 17 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 18 % Show Material materials with Elongation of 18 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
Hardness, Brinell | 268 [-] Show Material materials with Hardness, Brinell of 268 [-] | Predicted Value, Transverse | ||||
Poisson's ratio | 20 °C | 0.284 [-] Show Material materials with Poisson's ratio of 0.284 [-] | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | |
Reduction of area | 42.3 % Show Material materials with Reduction of area of 42.3 % | Predicted Value, Transverse | ||||
51.8 % Show Material materials with Reduction of area of 51.8 % | Predicted Value | |||||
Shear modulus | 82 GPa Show Material materials with Shear modulus of 82 GPa | Typical for Low Carbon Steel | ||||
Shear strength | 636.4 MPa Show Material materials with Shear strength of 636.4 MPa | Predicted Value | ||||
Tensile strength | 20 °C | 270 - 540 MPa Show Material materials with Tensile strength of 270 - 540 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | |
20 °C | 270 - 510 MPa Show Material materials with Tensile strength of 270 - 510 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 270 - 500 MPa Show Material materials with Tensile strength of 270 - 500 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 270 - 490 MPa Show Material materials with Tensile strength of 270 - 490 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 280 - 540 MPa Show Material materials with Tensile strength of 280 - 540 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 280 - 510 MPa Show Material materials with Tensile strength of 280 - 510 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 280 - 500 MPa Show Material materials with Tensile strength of 280 - 500 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 280 - 490 MPa Show Material materials with Tensile strength of 280 - 490 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 290 - 540 MPa Show Material materials with Tensile strength of 290 - 540 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 290 - 510 MPa Show Material materials with Tensile strength of 290 - 510 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 290 - 500 MPa Show Material materials with Tensile strength of 290 - 500 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 290 - 490 MPa Show Material materials with Tensile strength of 290 - 490 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 310 - 540 MPa Show Material materials with Tensile strength of 310 - 540 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 310 - 510 MPa Show Material materials with Tensile strength of 310 - 510 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 310 - 500 MPa Show Material materials with Tensile strength of 310 - 500 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 310 - 490 MPa Show Material materials with Tensile strength of 310 - 490 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
Yield strength | 271.7 MPa Show Material materials with Yield strength of 271.7 MPa | Predicted Value, RP1 | ||||
282.3 MPa Show Material materials with Yield strength of 282.3 MPa | Predicted Value, Transverse | |||||
303.2 MPa Show Material materials with Yield strength of 303.2 MPa | Predicted Value, RP05 | |||||
311.9 MPa Show Material materials with Yield strength of 311.9 MPa | Predicted Value, RP1 Transverse | |||||
373.1 MPa Show Material materials with Yield strength of 373.1 MPa | Predicted Value, RP02 | |||||
496.3 MPa Show Material materials with Yield strength of 496.3 MPa | Predicted Value, RP02 Transverse | |||||
500.2 MPa Show Material materials with Yield strength of 500.2 MPa | Predicted Value, RP002 | |||||
20 °C | 145 MPa Show Material materials with Yield strength of 145 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 155 MPa Show Material materials with Yield strength of 155 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 165 MPa Show Material materials with Yield strength of 165 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 175 MPa Show Material materials with Yield strength of 175 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 185 MPa Show Material materials with Yield strength of 185 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire |
Thermal
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Coefficient of thermal expansion | -100 °C | 1.08e-05 1/K Show Material materials with Coefficient of thermal expansion of 1.08e-05 1/K | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | |
20 °C | 1.19e-05 1/K Show Material materials with Coefficient of thermal expansion of 1.19e-05 1/K | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
100 °C | 1.25e-05 1/K Show Material materials with Coefficient of thermal expansion of 1.25e-05 1/K | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
200 °C | 1.3e-05 1/K Show Material materials with Coefficient of thermal expansion of 1.3e-05 1/K | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
300 °C | 1.36e-05 1/K Show Material materials with Coefficient of thermal expansion of 1.36e-05 1/K | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
400 °C | 1.41e-05 1/K Show Material materials with Coefficient of thermal expansion of 1.41e-05 1/K | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
500 °C | 1.45e-05 1/K Show Material materials with Coefficient of thermal expansion of 1.45e-05 1/K | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
600 °C | 1.49e-05 1/K Show Material materials with Coefficient of thermal expansion of 1.49e-05 1/K | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
Max service temperature | 400.7 °C Show Material materials with Max service temperature of 400.7 °C | Predicted Value, Long | ||||
500 °C Show Material materials with Max service temperature of 500 °C | Typical for Carbon Steel | |||||
Melting point | 1480 - 1526 °C Show Material materials with Melting point of 1480 - 1526 °C | Typical for Low Carbon Steel | ||||
Specific heat capacity | -100 °C | 423 J/(kg·K) Show Material materials with Specific heat capacity of 423 J/(kg·K) | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | |
20 °C | 461 J/(kg·K) Show Material materials with Specific heat capacity of 461 J/(kg·K) | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
100 °C | 479 J/(kg·K) Show Material materials with Specific heat capacity of 479 J/(kg·K) | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
200 °C | 499 J/(kg·K) Show Material materials with Specific heat capacity of 499 J/(kg·K) | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
300 °C | 517 J/(kg·K) Show Material materials with Specific heat capacity of 517 J/(kg·K) | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
400 °C | 536 J/(kg·K) Show Material materials with Specific heat capacity of 536 J/(kg·K) | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
500 °C | 558 J/(kg·K) Show Material materials with Specific heat capacity of 558 J/(kg·K) | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
600 °C | 587 J/(kg·K) Show Material materials with Specific heat capacity of 587 J/(kg·K) | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
Thermal conductivity | 20 °C | 56.9 W/(m·K) Show Material materials with Thermal conductivity of 56.9 W/(m·K) | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | |
100 °C | 56.4 W/(m·K) Show Material materials with Thermal conductivity of 56.4 W/(m·K) | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
200 °C | 53.5 W/(m·K) Show Material materials with Thermal conductivity of 53.5 W/(m·K) | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
300 °C | 49.4 W/(m·K) Show Material materials with Thermal conductivity of 49.4 W/(m·K) | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
400 °C | 45.2 W/(m·K) Show Material materials with Thermal conductivity of 45.2 W/(m·K) | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
500 °C | 41.3 W/(m·K) Show Material materials with Thermal conductivity of 41.3 W/(m·K) | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
600 °C | 37.6 W/(m·K) Show Material materials with Thermal conductivity of 37.6 W/(m·K) | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
Thermal diffusivity | 20 °C | 15.7 mm²/s Show Material materials with Thermal diffusivity of 15.7 mm²/s | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | |
100 °C | 14.5 mm²/s Show Material materials with Thermal diffusivity of 14.5 mm²/s | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
200 °C | 12.9 mm²/s Show Material materials with Thermal diffusivity of 12.9 mm²/s | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
300 °C | 11.2 mm²/s Show Material materials with Thermal diffusivity of 11.2 mm²/s | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
400 °C | 9.6 mm²/s Show Material materials with Thermal diffusivity of 9.6 mm²/s | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
500 °C | 7.9 mm²/s Show Material materials with Thermal diffusivity of 7.9 mm²/s | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
600 °C | 6.3 mm²/s Show Material materials with Thermal diffusivity of 6.3 mm²/s | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire |
Electrical
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Electrical conductivity | 8 S/m Show Material materials with Electrical conductivity of 8 S/m | Predicted Value | ||||
Electrical resistivity | 20 °C | 1.83e-07 Ω·m Show Material materials with Electrical resistivity of 1.83e-07 Ω·m | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | |
100 °C | 2.27e-07 Ω·m Show Material materials with Electrical resistivity of 2.27e-07 Ω·m | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
200 °C | 2.95e-07 Ω·m Show Material materials with Electrical resistivity of 2.95e-07 Ω·m | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
300 °C | 3.8e-07 Ω·m Show Material materials with Electrical resistivity of 3.8e-07 Ω·m | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
400 °C | 4.81e-07 Ω·m Show Material materials with Electrical resistivity of 4.81e-07 Ω·m | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
500 °C | 5.99e-07 Ω·m Show Material materials with Electrical resistivity of 5.99e-07 Ω·m | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
600 °C | 7.38e-07 Ω·m Show Material materials with Electrical resistivity of 7.38e-07 Ω·m | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire |
Magnetic
Property | Value | Comment |
---|---|---|
Curie temperature | 770 °C Show Material materials with Curie temperature of 770 °C | Typical for Low Carbon Steel |
Do you have a technical question or need more information about this material?
Post it as a comment below and receive answers from engineers and other community members.