EN 10025-2 Grade S235JR as-rolled condition (+AR)

View suppliers (83)
Want to keep this datasheet? Save it now in your required format

Description

S235JR is applicated for construction parts of moderate strength load, which are not liable to inspection. Max. product thickness accounts for 25 mm. For this steel are available (see material No. 1.0120 acc. to DIN EN 10025) grades for: - folding (KQ)-S235JRC - cold forming of sections (KP)-S235JRC - cold drawing (KZ)-S235JRC

Related Standards

Equivalent Materials

This material data has been provided by WIAM.

"Typical" values were obtained via a literature search. "Predicted" values were imputed via artificial intelligence technology. While we have placed significant efforts in ensuring data accuracy, "typical" and "predicted" data should be considered indicative and verified by appropriate material testing. Please do contact us if additional information on the the predicted data method is required.
All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValueConditionRelated StandardsShape

Density

20 °C

7.85 g/cm³

Show Material materials with Density of 7.85 g/cm³

as-rolled condition (+AR)

EN 10025, EN 10025-1, EN 10025-2

Sheet, Strip, Flat

Mechanical

PropertyTemperatureValueConditionRelated StandardsShapeComment

Elastic modulus

-100 °C

217 GPa

Show Material materials with Elastic modulus of 217 GPa

as-rolled condition (+AR)

EN 10025, EN 10025-1, EN 10025-2

Sheet, Strip, Flat

20 °C

212 GPa

Show Material materials with Elastic modulus of 212 GPa

as-rolled condition (+AR)

EN 10025, EN 10025-1, EN 10025-2

Sheet, Strip, Flat

100 °C

207 GPa

Show Material materials with Elastic modulus of 207 GPa

as-rolled condition (+AR)

EN 10025, EN 10025-1, EN 10025-2

Sheet, Strip, Flat

200 °C

199 GPa

Show Material materials with Elastic modulus of 199 GPa

as-rolled condition (+AR)

EN 10025, EN 10025-1, EN 10025-2

Sheet, Strip, Flat

300 °C

192 GPa

Show Material materials with Elastic modulus of 192 GPa

as-rolled condition (+AR)

EN 10025, EN 10025-1, EN 10025-2

Sheet, Strip, Flat

400 °C

184 GPa

Show Material materials with Elastic modulus of 184 GPa

as-rolled condition (+AR)

EN 10025, EN 10025-1, EN 10025-2

Sheet, Strip, Flat

500 °C

175 GPa

Show Material materials with Elastic modulus of 175 GPa

as-rolled condition (+AR)

EN 10025, EN 10025-1, EN 10025-2

Sheet, Strip, Flat

600 °C

164 GPa

Show Material materials with Elastic modulus of 164 GPa

as-rolled condition (+AR)

EN 10025, EN 10025-1, EN 10025-2

Sheet, Strip, Flat

Elongation

18.0 %

Show Material materials with Elongation of 18.0 %

Predicted Value, A200

18.3 %

Show Material materials with Elongation of 18.3 %

Predicted Value, A80 Transverse

19 %

Show Material materials with Elongation of 19 %

Predicted Value, Transverse

22.1 %

Show Material materials with Elongation of 22.1 %

Predicted Value, A5

24.8 %

Show Material materials with Elongation of 24.8 %

Predicted Value, A50

25.2 %

Show Material materials with Elongation of 25.2 %

Predicted Value

20 °C

17 %

Show Material materials with Elongation of 17 %

as-rolled condition (+AR)

EN 10025, EN 10025-1, EN 10025-2

Sheet, Strip, Flat

A80

20 °C

18 %

Show Material materials with Elongation of 18 %

as-rolled condition (+AR)

EN 10025, EN 10025-1, EN 10025-2

Sheet, Strip, Flat

A80

20 °C

19 %

Show Material materials with Elongation of 19 %

as-rolled condition (+AR)

EN 10025, EN 10025-1, EN 10025-2

Sheet, Strip, Flat

A80

20 °C

20 %

Show Material materials with Elongation of 20 %

as-rolled condition (+AR)

EN 10025, EN 10025-1, EN 10025-2

Sheet, Strip, Flat

A80

20 °C

21 %

Show Material materials with Elongation of 21 %

as-rolled condition (+AR)

EN 10025, EN 10025-1, EN 10025-2

Sheet, Strip, Flat

A80

Hardness, Brinell

247 [-]

Show Material materials with Hardness, Brinell of 247 [-]

Predicted Value, Transverse

Poisson's ratio

20 °C

0.284 [-]

Show Material materials with Poisson's ratio of 0.284 [-]

as-rolled condition (+AR)

EN 10025, EN 10025-1, EN 10025-2

Sheet, Strip, Flat

Reduction of area

42.1 %

Show Material materials with Reduction of area of 42.1 %

Predicted Value

43.4 %

Show Material materials with Reduction of area of 43.4 %

Predicted Value, Transverse

Shear modulus

82 GPa

Show Material materials with Shear modulus of 82 GPa

Typical for Low Carbon Steel

Shear strength

510 MPa

Show Material materials with Shear strength of 510 MPa

Predicted Value

Tensile strength

20 °C

340 - 510 MPa

Show Material materials with Tensile strength of 340 - 510 MPa

as-rolled condition (+AR)

EN 10025, EN 10025-1, EN 10025-2

Sheet, Strip, Flat

20 °C

340 - 470 MPa

Show Material materials with Tensile strength of 340 - 470 MPa

as-rolled condition (+AR)

EN 10025, EN 10025-1, EN 10025-2

Sheet, Strip, Flat

20 °C

360 - 510 MPa

Show Material materials with Tensile strength of 360 - 510 MPa

as-rolled condition (+AR)

EN 10025, EN 10025-1, EN 10025-2

Sheet, Strip, Flat

20 °C

360 - 470 MPa

Show Material materials with Tensile strength of 360 - 470 MPa

as-rolled condition (+AR)

EN 10025, EN 10025-1, EN 10025-2

Sheet, Strip, Flat

Yield strength

260 MPa

Show Material materials with Yield strength of 260 MPa

Predicted Value, RP1

292.7 MPa

Show Material materials with Yield strength of 292.7 MPa

Predicted Value, Transverse

294.7 MPa

Show Material materials with Yield strength of 294.7 MPa

Predicted Value, RP05

318.2 MPa

Show Material materials with Yield strength of 318.2 MPa

Predicted Value, RP1 Transverse

336.3 MPa

Show Material materials with Yield strength of 336.3 MPa

Predicted Value, RP02

469.3 MPa

Show Material materials with Yield strength of 469.3 MPa

Predicted Value, RP02 Transverse

477.1 MPa

Show Material materials with Yield strength of 477.1 MPa

Predicted Value, RP002

20 °C

225 MPa

Show Material materials with Yield strength of 225 MPa

as-rolled condition (+AR)

EN 10025, EN 10025-1, EN 10025-2

Sheet, Strip, Flat

20 °C

235 MPa

Show Material materials with Yield strength of 235 MPa

as-rolled condition (+AR)

EN 10025, EN 10025-1, EN 10025-2

Sheet, Strip, Flat

Thermal

PropertyTemperatureValueConditionRelated StandardsShapeComment

Coefficient of thermal expansion

-100 °C

1.08e-05 1/K

Show Material materials with Coefficient of thermal expansion of 1.08e-05 1/K

as-rolled condition (+AR)

EN 10025, EN 10025-1, EN 10025-2

Sheet, Strip, Flat

20 °C

1.19e-05 1/K

Show Material materials with Coefficient of thermal expansion of 1.19e-05 1/K

as-rolled condition (+AR)

EN 10025, EN 10025-1, EN 10025-2

Sheet, Strip, Flat

100 °C

1.25e-05 1/K

Show Material materials with Coefficient of thermal expansion of 1.25e-05 1/K

as-rolled condition (+AR)

EN 10025, EN 10025-1, EN 10025-2

Sheet, Strip, Flat

200 °C

1.3e-05 1/K

Show Material materials with Coefficient of thermal expansion of 1.3e-05 1/K

as-rolled condition (+AR)

EN 10025, EN 10025-1, EN 10025-2

Sheet, Strip, Flat

300 °C

1.36e-05 1/K

Show Material materials with Coefficient of thermal expansion of 1.36e-05 1/K

as-rolled condition (+AR)

EN 10025, EN 10025-1, EN 10025-2

Sheet, Strip, Flat

400 °C

1.41e-05 1/K

Show Material materials with Coefficient of thermal expansion of 1.41e-05 1/K

as-rolled condition (+AR)

EN 10025, EN 10025-1, EN 10025-2

Sheet, Strip, Flat

500 °C

1.45e-05 1/K

Show Material materials with Coefficient of thermal expansion of 1.45e-05 1/K

as-rolled condition (+AR)

EN 10025, EN 10025-1, EN 10025-2

Sheet, Strip, Flat

600 °C

1.49e-05 1/K

Show Material materials with Coefficient of thermal expansion of 1.49e-05 1/K

as-rolled condition (+AR)

EN 10025, EN 10025-1, EN 10025-2

Sheet, Strip, Flat

Max service temperature

391.1 °C

Show Material materials with Max service temperature of 391.1 °C

Predicted Value, Long

500 °C

Show Material materials with Max service temperature of 500 °C

Typical for Carbon Steel

Melting point

1480 - 1526 °C

Show Material materials with Melting point of 1480 - 1526 °C

Typical for Low Carbon Steel

Specific heat capacity

-100 °C

423 J/(kg·K)

Show Material materials with Specific heat capacity of 423 J/(kg·K)

as-rolled condition (+AR)

EN 10025, EN 10025-1, EN 10025-2

Sheet, Strip, Flat

20 °C

461 J/(kg·K)

Show Material materials with Specific heat capacity of 461 J/(kg·K)

as-rolled condition (+AR)

EN 10025, EN 10025-1, EN 10025-2

Sheet, Strip, Flat

100 °C

479 J/(kg·K)

Show Material materials with Specific heat capacity of 479 J/(kg·K)

as-rolled condition (+AR)

EN 10025, EN 10025-1, EN 10025-2

Sheet, Strip, Flat

200 °C

499 J/(kg·K)

Show Material materials with Specific heat capacity of 499 J/(kg·K)

as-rolled condition (+AR)

EN 10025, EN 10025-1, EN 10025-2

Sheet, Strip, Flat

300 °C

517 J/(kg·K)

Show Material materials with Specific heat capacity of 517 J/(kg·K)

as-rolled condition (+AR)

EN 10025, EN 10025-1, EN 10025-2

Sheet, Strip, Flat

400 °C

536 J/(kg·K)

Show Material materials with Specific heat capacity of 536 J/(kg·K)

as-rolled condition (+AR)

EN 10025, EN 10025-1, EN 10025-2

Sheet, Strip, Flat

500 °C

558 J/(kg·K)

Show Material materials with Specific heat capacity of 558 J/(kg·K)

as-rolled condition (+AR)

EN 10025, EN 10025-1, EN 10025-2

Sheet, Strip, Flat

600 °C

587 J/(kg·K)

Show Material materials with Specific heat capacity of 587 J/(kg·K)

as-rolled condition (+AR)

EN 10025, EN 10025-1, EN 10025-2

Sheet, Strip, Flat

Thermal conductivity

20 °C

56.9 W/(m·K)

Show Material materials with Thermal conductivity of 56.9 W/(m·K)

as-rolled condition (+AR)

EN 10025, EN 10025-1, EN 10025-2

Sheet, Strip, Flat

100 °C

56.4 W/(m·K)

Show Material materials with Thermal conductivity of 56.4 W/(m·K)

as-rolled condition (+AR)

EN 10025, EN 10025-1, EN 10025-2

Sheet, Strip, Flat

200 °C

53.5 W/(m·K)

Show Material materials with Thermal conductivity of 53.5 W/(m·K)

as-rolled condition (+AR)

EN 10025, EN 10025-1, EN 10025-2

Sheet, Strip, Flat

300 °C

49.4 W/(m·K)

Show Material materials with Thermal conductivity of 49.4 W/(m·K)

as-rolled condition (+AR)

EN 10025, EN 10025-1, EN 10025-2

Sheet, Strip, Flat

400 °C

45.2 W/(m·K)

Show Material materials with Thermal conductivity of 45.2 W/(m·K)

as-rolled condition (+AR)

EN 10025, EN 10025-1, EN 10025-2

Sheet, Strip, Flat

500 °C

41.3 W/(m·K)

Show Material materials with Thermal conductivity of 41.3 W/(m·K)

as-rolled condition (+AR)

EN 10025, EN 10025-1, EN 10025-2

Sheet, Strip, Flat

600 °C

37.6 W/(m·K)

Show Material materials with Thermal conductivity of 37.6 W/(m·K)

as-rolled condition (+AR)

EN 10025, EN 10025-1, EN 10025-2

Sheet, Strip, Flat

Thermal diffusivity

20 °C

15.7 mm²/s

Show Material materials with Thermal diffusivity of 15.7 mm²/s

as-rolled condition (+AR)

EN 10025, EN 10025-1, EN 10025-2

Sheet, Strip, Flat

100 °C

14.5 mm²/s

Show Material materials with Thermal diffusivity of 14.5 mm²/s

as-rolled condition (+AR)

EN 10025, EN 10025-1, EN 10025-2

Sheet, Strip, Flat

200 °C

12.9 mm²/s

Show Material materials with Thermal diffusivity of 12.9 mm²/s

as-rolled condition (+AR)

EN 10025, EN 10025-1, EN 10025-2

Sheet, Strip, Flat

300 °C

11.2 mm²/s

Show Material materials with Thermal diffusivity of 11.2 mm²/s

as-rolled condition (+AR)

EN 10025, EN 10025-1, EN 10025-2

Sheet, Strip, Flat

400 °C

9.6 mm²/s

Show Material materials with Thermal diffusivity of 9.6 mm²/s

as-rolled condition (+AR)

EN 10025, EN 10025-1, EN 10025-2

Sheet, Strip, Flat

500 °C

7.9 mm²/s

Show Material materials with Thermal diffusivity of 7.9 mm²/s

as-rolled condition (+AR)

EN 10025, EN 10025-1, EN 10025-2

Sheet, Strip, Flat

600 °C

6.3 mm²/s

Show Material materials with Thermal diffusivity of 6.3 mm²/s

as-rolled condition (+AR)

EN 10025, EN 10025-1, EN 10025-2

Sheet, Strip, Flat

Electrical

PropertyTemperatureValueConditionRelated StandardsShapeComment

Electrical conductivity

8 S/m

Show Material materials with Electrical conductivity of 8 S/m

Predicted Value

Electrical resistivity

20 °C

1.83e-07 Ω·m

Show Material materials with Electrical resistivity of 1.83e-07 Ω·m

as-rolled condition (+AR)

EN 10025, EN 10025-1, EN 10025-2

Sheet, Strip, Flat

100 °C

2.27e-07 Ω·m

Show Material materials with Electrical resistivity of 2.27e-07 Ω·m

as-rolled condition (+AR)

EN 10025, EN 10025-1, EN 10025-2

Sheet, Strip, Flat

200 °C

2.95e-07 Ω·m

Show Material materials with Electrical resistivity of 2.95e-07 Ω·m

as-rolled condition (+AR)

EN 10025, EN 10025-1, EN 10025-2

Sheet, Strip, Flat

300 °C

3.8e-07 Ω·m

Show Material materials with Electrical resistivity of 3.8e-07 Ω·m

as-rolled condition (+AR)

EN 10025, EN 10025-1, EN 10025-2

Sheet, Strip, Flat

400 °C

4.81e-07 Ω·m

Show Material materials with Electrical resistivity of 4.81e-07 Ω·m

as-rolled condition (+AR)

EN 10025, EN 10025-1, EN 10025-2

Sheet, Strip, Flat

500 °C

5.99e-07 Ω·m

Show Material materials with Electrical resistivity of 5.99e-07 Ω·m

as-rolled condition (+AR)

EN 10025, EN 10025-1, EN 10025-2

Sheet, Strip, Flat

600 °C

7.38e-07 Ω·m

Show Material materials with Electrical resistivity of 7.38e-07 Ω·m

as-rolled condition (+AR)

EN 10025, EN 10025-1, EN 10025-2

Sheet, Strip, Flat

Magnetic

PropertyValueComment

Curie temperature

770 °C

Show Material materials with Curie temperature of 770 °C

Typical for Low Carbon Steel

Chemical properties

PropertyValueConditionRelated StandardsShape

Carbon

0.17 %

Show Material materials with Carbon of 0.17 %

as-rolled condition (+AR)

EN 10025, EN 10025-1, EN 10025-2

Sheet, Strip, Flat

Manganese

1.4 %

Show Material materials with Manganese of 1.4 %

as-rolled condition (+AR)

EN 10025, EN 10025-1, EN 10025-2

Sheet, Strip, Flat

Nitrogen

0.009 %

Show Material materials with Nitrogen of 0.009 %

as-rolled condition (+AR)

EN 10025, EN 10025-1, EN 10025-2

Sheet, Strip, Flat

Phosphorus

0.045 %

Show Material materials with Phosphorus of 0.045 %

as-rolled condition (+AR)

EN 10025, EN 10025-1, EN 10025-2

Sheet, Strip, Flat

Sulfur

0.045 %

Show Material materials with Sulfur of 0.045 %

as-rolled condition (+AR)

EN 10025, EN 10025-1, EN 10025-2

Sheet, Strip, Flat

Do you have a technical question or need more information about this material?