The hot rolled, unalloyed quality steel S355JR is a higher strength fine grained steel for steel structural engineering. Dimensioning advantages in respect to the S235JR due to the by 120 MPa higher yield strength. The steel shows a by 15% higher resistance to mineral wear due to sliding action in comparison to S235JR. The steel is not intended for heat treatment. Stress relieving annealing is allowed. Products in the delivery condition +N may be hot formed and/or normalized after delivery. For long products and continuous rolled flats the delivery condition is up to the producer +AR, +N or +M. The delivery condition of four-high rolled sheet is also up to the producer and may be +AR or +N. Both conditions can be ordered. For this steel is available (mat. no 1.0551, S355JRC) a grade for cold drawing.

Related Standards

Equivalent Materials

This material data has been provided by WIAM.

"Typical" values were obtained via a literature search. "Predicted" values were imputed via artificial intelligence technology. While we have placed significant efforts in ensuring data accuracy, "typical" and "predicted" data should be considered indicative and verified by appropriate material testing. Please do contact us if additional information on the the predicted data method is required.
All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValueConditionRelated StandardsShape

Density

20 °C

7.83 g/cm³

Show Material materials with Density of 7.83 g/cm³

normalized or normalized formed (+N)

EN 10025-2, EN 10025

Strip, Sheet, Flat, Rod, Wire

Mechanical

PropertyTemperatureValueConditionRelated StandardsShapeComment

Elastic modulus

-100 °C

217 GPa

Show Material materials with Elastic modulus of 217 GPa

normalized or normalized formed (+N)

EN 10025-2, EN 10025

Strip, Sheet, Flat, Rod, Wire

20 °C

212 GPa

Show Material materials with Elastic modulus of 212 GPa

normalized or normalized formed (+N)

EN 10025-2, EN 10025

Strip, Sheet, Flat, Rod, Wire

100 °C

207 GPa

Show Material materials with Elastic modulus of 207 GPa

normalized or normalized formed (+N)

EN 10025-2, EN 10025

Strip, Sheet, Flat, Rod, Wire

200 °C

199 GPa

Show Material materials with Elastic modulus of 199 GPa

normalized or normalized formed (+N)

EN 10025-2, EN 10025

Strip, Sheet, Flat, Rod, Wire

300 °C

192 GPa

Show Material materials with Elastic modulus of 192 GPa

normalized or normalized formed (+N)

EN 10025-2, EN 10025

Strip, Sheet, Flat, Rod, Wire

400 °C

184 GPa

Show Material materials with Elastic modulus of 184 GPa

normalized or normalized formed (+N)

EN 10025-2, EN 10025

Strip, Sheet, Flat, Rod, Wire

500 °C

175 GPa

Show Material materials with Elastic modulus of 175 GPa

normalized or normalized formed (+N)

EN 10025-2, EN 10025

Strip, Sheet, Flat, Rod, Wire

600 °C

164 GPa

Show Material materials with Elastic modulus of 164 GPa

normalized or normalized formed (+N)

EN 10025-2, EN 10025

Strip, Sheet, Flat, Rod, Wire

Elongation

17.2 %

Show Material materials with Elongation of 17.2 %

Predicted Value, A200

19.3 %

Show Material materials with Elongation of 19.3 %

Predicted Value, A50

22.4 %

Show Material materials with Elongation of 22.4 %

Predicted Value, A5

20 °C

12 %

Show Material materials with Elongation of 12 %

normalized or normalized formed (+N)

EN 10025-2, EN 10025

Strip, Sheet, Flat, Rod, Wire

A80 Transverse

20 °C

13 %

Show Material materials with Elongation of 13 %

normalized or normalized formed (+N)

EN 10025-2, EN 10025

Strip, Sheet, Flat, Rod, Wire

A80 Transverse

20 °C

14 %

Show Material materials with Elongation of 14 %

normalized or normalized formed (+N)

EN 10025-2, EN 10025

Strip, Sheet, Flat, Rod, Wire

A80 Transverse

20 °C

14 %

Show Material materials with Elongation of 14 %

normalized or normalized formed (+N)

EN 10025-2, EN 10025

Strip, Sheet, Flat, Rod, Wire

A80

20 °C

15 %

Show Material materials with Elongation of 15 %

normalized or normalized formed (+N)

EN 10025-2, EN 10025

Strip, Sheet, Flat, Rod, Wire

A80 Transverse

20 °C

15 %

Show Material materials with Elongation of 15 %

normalized or normalized formed (+N)

EN 10025-2, EN 10025

Strip, Sheet, Flat, Rod, Wire

A80

20 °C

16 %

Show Material materials with Elongation of 16 %

normalized or normalized formed (+N)

EN 10025-2, EN 10025

Strip, Sheet, Flat, Rod, Wire

A80 Transverse

20 °C

16 %

Show Material materials with Elongation of 16 %

normalized or normalized formed (+N)

EN 10025-2, EN 10025

Strip, Sheet, Flat, Rod, Wire

A80

20 °C

17 %

Show Material materials with Elongation of 17 %

normalized or normalized formed (+N)

EN 10025-2, EN 10025

Strip, Sheet, Flat, Rod, Wire

A80

20 °C

17 %

Show Material materials with Elongation of 17 %

normalized or normalized formed (+N)

EN 10025-2, EN 10025

Strip, Sheet, Flat, Rod, Wire

Transverse

20 °C

17 %

Show Material materials with Elongation of 17 %

normalized or normalized formed (+N)

EN 10025-2, EN 10025

Strip, Sheet, Flat, Rod, Wire

20 °C

18 %

Show Material materials with Elongation of 18 %

normalized or normalized formed (+N)

EN 10025-2, EN 10025

Strip, Sheet, Flat, Rod, Wire

A80

20 °C

18 %

Show Material materials with Elongation of 18 %

normalized or normalized formed (+N)

EN 10025-2, EN 10025

Strip, Sheet, Flat, Rod, Wire

Transverse

20 °C

18 %

Show Material materials with Elongation of 18 %

normalized or normalized formed (+N)

EN 10025-2, EN 10025

Strip, Sheet, Flat, Rod, Wire

20 °C

19 %

Show Material materials with Elongation of 19 %

normalized or normalized formed (+N)

EN 10025-2, EN 10025

Strip, Sheet, Flat, Rod, Wire

Transverse

20 °C

20 %

Show Material materials with Elongation of 20 %

normalized or normalized formed (+N)

EN 10025-2, EN 10025

Strip, Sheet, Flat, Rod, Wire

Transverse

20 °C

20 %

Show Material materials with Elongation of 20 %

normalized or normalized formed (+N)

EN 10025-2, EN 10025

Strip, Sheet, Flat, Rod, Wire

20 °C

21 %

Show Material materials with Elongation of 21 %

normalized or normalized formed (+N)

EN 10025-2, EN 10025

Strip, Sheet, Flat, Rod, Wire

20 °C

22 %

Show Material materials with Elongation of 22 %

normalized or normalized formed (+N)

EN 10025-2, EN 10025

Strip, Sheet, Flat, Rod, Wire

Hardness, Brinell

243 [-]

Show Material materials with Hardness, Brinell of 243 [-]

Predicted Value, Transverse

Poisson's ratio

0.29 [-]

Show Material materials with Poisson's ratio of 0.29 [-]

Typical for Low Carbon Steel

Reduction of area

44.2 %

Show Material materials with Reduction of area of 44.2 %

Predicted Value, Transverse

51.7 %

Show Material materials with Reduction of area of 51.7 %

Predicted Value

Shear modulus

82 GPa

Show Material materials with Shear modulus of 82 GPa

Typical for Low Carbon Steel

Shear strength

510.2 MPa

Show Material materials with Shear strength of 510.2 MPa

Predicted Value

Tensile strength

20 °C

450 - 680 MPa

Show Material materials with Tensile strength of 450 - 680 MPa

normalized or normalized formed (+N)

EN 10025-2, EN 10025

Strip, Sheet, Flat, Rod, Wire

20 °C

450 - 630 MPa

Show Material materials with Tensile strength of 450 - 630 MPa

normalized or normalized formed (+N)

EN 10025-2, EN 10025

Strip, Sheet, Flat, Rod, Wire

20 °C

450 - 600 MPa

Show Material materials with Tensile strength of 450 - 600 MPa

normalized or normalized formed (+N)

EN 10025-2, EN 10025

Strip, Sheet, Flat, Rod, Wire

20 °C

470 - 680 MPa

Show Material materials with Tensile strength of 470 - 680 MPa

normalized or normalized formed (+N)

EN 10025-2, EN 10025

Strip, Sheet, Flat, Rod, Wire

20 °C

470 - 630 MPa

Show Material materials with Tensile strength of 470 - 630 MPa

normalized or normalized formed (+N)

EN 10025-2, EN 10025

Strip, Sheet, Flat, Rod, Wire

20 °C

470 - 600 MPa

Show Material materials with Tensile strength of 470 - 600 MPa

normalized or normalized formed (+N)

EN 10025-2, EN 10025

Strip, Sheet, Flat, Rod, Wire

20 °C

510 - 680 MPa

Show Material materials with Tensile strength of 510 - 680 MPa

normalized or normalized formed (+N)

EN 10025-2, EN 10025

Strip, Sheet, Flat, Rod, Wire

20 °C

510 - 630 MPa

Show Material materials with Tensile strength of 510 - 630 MPa

normalized or normalized formed (+N)

EN 10025-2, EN 10025

Strip, Sheet, Flat, Rod, Wire

20 °C

510 - 600 MPa

Show Material materials with Tensile strength of 510 - 600 MPa

normalized or normalized formed (+N)

EN 10025-2, EN 10025

Strip, Sheet, Flat, Rod, Wire

Yield strength

243.8 MPa

Show Material materials with Yield strength of 243.8 MPa

Predicted Value, RP1

309.3 MPa

Show Material materials with Yield strength of 309.3 MPa

Predicted Value, RP1 Transverse

364 MPa

Show Material materials with Yield strength of 364 MPa

Predicted Value, Transverse

384.7 MPa

Show Material materials with Yield strength of 384.7 MPa

Predicted Value, RP05

403.7 MPa

Show Material materials with Yield strength of 403.7 MPa

Predicted Value, RP02

474.7 MPa

Show Material materials with Yield strength of 474.7 MPa

Predicted Value, RP02 Transverse

480.2 MPa

Show Material materials with Yield strength of 480.2 MPa

Predicted Value, RP002

20 °C

275 MPa

Show Material materials with Yield strength of 275 MPa

normalized or normalized formed (+N)

EN 10025-2, EN 10025

Strip, Sheet, Flat, Rod, Wire

20 °C

285 MPa

Show Material materials with Yield strength of 285 MPa

normalized or normalized formed (+N)

EN 10025-2, EN 10025

Strip, Sheet, Flat, Rod, Wire

20 °C

295 MPa

Show Material materials with Yield strength of 295 MPa

normalized or normalized formed (+N)

EN 10025-2, EN 10025

Strip, Sheet, Flat, Rod, Wire

20 °C

315 MPa

Show Material materials with Yield strength of 315 MPa

normalized or normalized formed (+N)

EN 10025-2, EN 10025

Strip, Sheet, Flat, Rod, Wire

20 °C

325 MPa

Show Material materials with Yield strength of 325 MPa

normalized or normalized formed (+N)

EN 10025-2, EN 10025

Strip, Sheet, Flat, Rod, Wire

20 °C

335 MPa

Show Material materials with Yield strength of 335 MPa

normalized or normalized formed (+N)

EN 10025-2, EN 10025

Strip, Sheet, Flat, Rod, Wire

20 °C

345 MPa

Show Material materials with Yield strength of 345 MPa

normalized or normalized formed (+N)

EN 10025-2, EN 10025

Strip, Sheet, Flat, Rod, Wire

20 °C

355 MPa

Show Material materials with Yield strength of 355 MPa

normalized or normalized formed (+N)

EN 10025-2, EN 10025

Strip, Sheet, Flat, Rod, Wire

Thermal

PropertyTemperatureValueConditionRelated StandardsShapeComment

Coefficient of thermal expansion

-100 °C

1.08e-05 1/K

Show Material materials with Coefficient of thermal expansion of 1.08e-05 1/K

normalized or normalized formed (+N)

EN 10025-2, EN 10025

Strip, Sheet, Flat, Rod, Wire

20 °C

1.19e-05 1/K

Show Material materials with Coefficient of thermal expansion of 1.19e-05 1/K

normalized or normalized formed (+N)

EN 10025-2, EN 10025

Strip, Sheet, Flat, Rod, Wire

100 °C

1.25e-05 1/K

Show Material materials with Coefficient of thermal expansion of 1.25e-05 1/K

normalized or normalized formed (+N)

EN 10025-2, EN 10025

Strip, Sheet, Flat, Rod, Wire

200 °C

1.3e-05 1/K

Show Material materials with Coefficient of thermal expansion of 1.3e-05 1/K

normalized or normalized formed (+N)

EN 10025-2, EN 10025

Strip, Sheet, Flat, Rod, Wire

300 °C

1.36e-05 1/K

Show Material materials with Coefficient of thermal expansion of 1.36e-05 1/K

normalized or normalized formed (+N)

EN 10025-2, EN 10025

Strip, Sheet, Flat, Rod, Wire

400 °C

1.41e-05 1/K

Show Material materials with Coefficient of thermal expansion of 1.41e-05 1/K

normalized or normalized formed (+N)

EN 10025-2, EN 10025

Strip, Sheet, Flat, Rod, Wire

500 °C

1.45e-05 1/K

Show Material materials with Coefficient of thermal expansion of 1.45e-05 1/K

normalized or normalized formed (+N)

EN 10025-2, EN 10025

Strip, Sheet, Flat, Rod, Wire

600 °C

1.49e-05 1/K

Show Material materials with Coefficient of thermal expansion of 1.49e-05 1/K

normalized or normalized formed (+N)

EN 10025-2, EN 10025

Strip, Sheet, Flat, Rod, Wire

Max service temperature

360.4 °C

Show Material materials with Max service temperature of 360.4 °C

Predicted Value, Long

500 °C

Show Material materials with Max service temperature of 500 °C

Typical for Carbon Steel

Melting point

1480 - 1526 °C

Show Material materials with Melting point of 1480 - 1526 °C

Typical for Low Carbon Steel

Specific heat capacity

-100 °C

423 J/(kg·K)

Show Material materials with Specific heat capacity of 423 J/(kg·K)

normalized or normalized formed (+N)

EN 10025-2, EN 10025

Strip, Sheet, Flat, Rod, Wire

20 °C

461 J/(kg·K)

Show Material materials with Specific heat capacity of 461 J/(kg·K)

normalized or normalized formed (+N)

EN 10025-2, EN 10025

Strip, Sheet, Flat, Rod, Wire

100 °C

479 J/(kg·K)

Show Material materials with Specific heat capacity of 479 J/(kg·K)

normalized or normalized formed (+N)

EN 10025-2, EN 10025

Strip, Sheet, Flat, Rod, Wire

200 °C

499 J/(kg·K)

Show Material materials with Specific heat capacity of 499 J/(kg·K)

normalized or normalized formed (+N)

EN 10025-2, EN 10025

Strip, Sheet, Flat, Rod, Wire

300 °C

517 J/(kg·K)

Show Material materials with Specific heat capacity of 517 J/(kg·K)

normalized or normalized formed (+N)

EN 10025-2, EN 10025

Strip, Sheet, Flat, Rod, Wire

400 °C

536 J/(kg·K)

Show Material materials with Specific heat capacity of 536 J/(kg·K)

normalized or normalized formed (+N)

EN 10025-2, EN 10025

Strip, Sheet, Flat, Rod, Wire

500 °C

558 J/(kg·K)

Show Material materials with Specific heat capacity of 558 J/(kg·K)

normalized or normalized formed (+N)

EN 10025-2, EN 10025

Strip, Sheet, Flat, Rod, Wire

600 °C

587 J/(kg·K)

Show Material materials with Specific heat capacity of 587 J/(kg·K)

normalized or normalized formed (+N)

EN 10025-2, EN 10025

Strip, Sheet, Flat, Rod, Wire

Thermal conductivity

-100 °C

37.6 W/(m·K)

Show Material materials with Thermal conductivity of 37.6 W/(m·K)

normalized or normalized formed (+N)

EN 10025-2, EN 10025

Strip, Sheet, Flat, Rod, Wire

20 °C

42.2 W/(m·K)

Show Material materials with Thermal conductivity of 42.2 W/(m·K)

normalized or normalized formed (+N)

EN 10025-2, EN 10025

Strip, Sheet, Flat, Rod, Wire

100 °C

43.2 W/(m·K)

Show Material materials with Thermal conductivity of 43.2 W/(m·K)

normalized or normalized formed (+N)

EN 10025-2, EN 10025

Strip, Sheet, Flat, Rod, Wire

200 °C

42.9 W/(m·K)

Show Material materials with Thermal conductivity of 42.9 W/(m·K)

normalized or normalized formed (+N)

EN 10025-2, EN 10025

Strip, Sheet, Flat, Rod, Wire

300 °C

41.2 W/(m·K)

Show Material materials with Thermal conductivity of 41.2 W/(m·K)

normalized or normalized formed (+N)

EN 10025-2, EN 10025

Strip, Sheet, Flat, Rod, Wire

400 °C

39.1 W/(m·K)

Show Material materials with Thermal conductivity of 39.1 W/(m·K)

normalized or normalized formed (+N)

EN 10025-2, EN 10025

Strip, Sheet, Flat, Rod, Wire

500 °C

36.6 W/(m·K)

Show Material materials with Thermal conductivity of 36.6 W/(m·K)

normalized or normalized formed (+N)

EN 10025-2, EN 10025

Strip, Sheet, Flat, Rod, Wire

600 °C

34.1 W/(m·K)

Show Material materials with Thermal conductivity of 34.1 W/(m·K)

normalized or normalized formed (+N)

EN 10025-2, EN 10025

Strip, Sheet, Flat, Rod, Wire

Thermal diffusivity

-100 °C

12.9 mm²/s

Show Material materials with Thermal diffusivity of 12.9 mm²/s

normalized or normalized formed (+N)

EN 10025-2, EN 10025

Strip, Sheet, Flat, Rod, Wire

20 °C

11.7 mm²/s

Show Material materials with Thermal diffusivity of 11.7 mm²/s

normalized or normalized formed (+N)

EN 10025-2, EN 10025

Strip, Sheet, Flat, Rod, Wire

100 °C

11.2 mm²/s

Show Material materials with Thermal diffusivity of 11.2 mm²/s

normalized or normalized formed (+N)

EN 10025-2, EN 10025

Strip, Sheet, Flat, Rod, Wire

200 °C

10.3 mm²/s

Show Material materials with Thermal diffusivity of 10.3 mm²/s

normalized or normalized formed (+N)

EN 10025-2, EN 10025

Strip, Sheet, Flat, Rod, Wire

300 °C

9.4 mm²/s

Show Material materials with Thermal diffusivity of 9.4 mm²/s

normalized or normalized formed (+N)

EN 10025-2, EN 10025

Strip, Sheet, Flat, Rod, Wire

400 °C

8.3 mm²/s

Show Material materials with Thermal diffusivity of 8.3 mm²/s

normalized or normalized formed (+N)

EN 10025-2, EN 10025

Strip, Sheet, Flat, Rod, Wire

500 °C

7.1 mm²/s

Show Material materials with Thermal diffusivity of 7.1 mm²/s

normalized or normalized formed (+N)

EN 10025-2, EN 10025

Strip, Sheet, Flat, Rod, Wire

600 °C

5.7 mm²/s

Show Material materials with Thermal diffusivity of 5.7 mm²/s

normalized or normalized formed (+N)

EN 10025-2, EN 10025

Strip, Sheet, Flat, Rod, Wire

Electrical

PropertyTemperatureValueConditionRelated StandardsShapeComment

Electrical conductivity

8 S/m

Show Material materials with Electrical conductivity of 8 S/m

Predicted Value

Electrical resistivity

-100 °C

1.82e-07 Ω·m

Show Material materials with Electrical resistivity of 1.82e-07 Ω·m

normalized or normalized formed (+N)

EN 10025-2, EN 10025

Strip, Sheet, Flat, Rod, Wire

20 °C

2.47e-07 Ω·m

Show Material materials with Electrical resistivity of 2.47e-07 Ω·m

normalized or normalized formed (+N)

EN 10025-2, EN 10025

Strip, Sheet, Flat, Rod, Wire

100 °C

2.96e-07 Ω·m

Show Material materials with Electrical resistivity of 2.96e-07 Ω·m

normalized or normalized formed (+N)

EN 10025-2, EN 10025

Strip, Sheet, Flat, Rod, Wire

200 °C

3.68e-07 Ω·m

Show Material materials with Electrical resistivity of 3.68e-07 Ω·m

normalized or normalized formed (+N)

EN 10025-2, EN 10025

Strip, Sheet, Flat, Rod, Wire

300 °C

4.55e-07 Ω·m

Show Material materials with Electrical resistivity of 4.55e-07 Ω·m

normalized or normalized formed (+N)

EN 10025-2, EN 10025

Strip, Sheet, Flat, Rod, Wire

400 °C

5.56e-07 Ω·m

Show Material materials with Electrical resistivity of 5.56e-07 Ω·m

normalized or normalized formed (+N)

EN 10025-2, EN 10025

Strip, Sheet, Flat, Rod, Wire

500 °C

6.75e-07 Ω·m

Show Material materials with Electrical resistivity of 6.75e-07 Ω·m

normalized or normalized formed (+N)

EN 10025-2, EN 10025

Strip, Sheet, Flat, Rod, Wire

600 °C

8.13e-07 Ω·m

Show Material materials with Electrical resistivity of 8.13e-07 Ω·m

normalized or normalized formed (+N)

EN 10025-2, EN 10025

Strip, Sheet, Flat, Rod, Wire

Magnetic

PropertyValueComment

Curie temperature

770 °C

Show Material materials with Curie temperature of 770 °C

Typical for Low Carbon Steel

Chemical properties

PropertyValueConditionRelated StandardsShape

Carbon

0.24 %

Show Material materials with Carbon of 0.24 %

normalized or normalized formed (+N)

EN 10025-2, EN 10025

Strip, Sheet, Flat, Rod, Wire

Copper

0.55 %

Show Material materials with Copper of 0.55 %

normalized or normalized formed (+N)

EN 10025-2, EN 10025

Strip, Sheet, Flat, Rod, Wire

Manganese

1.6 %

Show Material materials with Manganese of 1.6 %

normalized or normalized formed (+N)

EN 10025-2, EN 10025

Strip, Sheet, Flat, Rod, Wire

Nitrogen

0.012 %

Show Material materials with Nitrogen of 0.012 %

normalized or normalized formed (+N)

EN 10025-2, EN 10025

Strip, Sheet, Flat, Rod, Wire

Phosphorus

0.035 %

Show Material materials with Phosphorus of 0.035 %

normalized or normalized formed (+N)

EN 10025-2, EN 10025

Strip, Sheet, Flat, Rod, Wire

Silicon

0.55 %

Show Material materials with Silicon of 0.55 %

normalized or normalized formed (+N)

EN 10025-2, EN 10025

Strip, Sheet, Flat, Rod, Wire

Sulfur

0.035 %

Show Material materials with Sulfur of 0.035 %

normalized or normalized formed (+N)

EN 10025-2, EN 10025

Strip, Sheet, Flat, Rod, Wire

Do you have a technical question or need more information about this material?

Post it as a comment below and receive answers from engineers and other community members.