General
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Density | 20 °C | 7.84 g/cm³ Show Material materials with Density of 7.84 g/cm³ | normalized and tempered (+NT) | EN 10028-2 | Flat |
Mechanical
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Elastic modulus | -100 °C | 217 GPa Show Material materials with Elastic modulus of 217 GPa | normalized and tempered (+NT) | EN 10028-2 | Flat | |
20 °C | 212 - 214 GPa Show Material materials with Elastic modulus of 212 - 214 GPa | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
20 °C | 212 GPa Show Material materials with Elastic modulus of 212 GPa | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
20 °C | 212 - 212.4 GPa Show Material materials with Elastic modulus of 212 - 212.4 GPa | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
20 °C | 212.4 - 214 GPa Show Material materials with Elastic modulus of 212.4 - 214 GPa | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
20 °C | 212.4 GPa Show Material materials with Elastic modulus of 212.4 GPa | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
20 °C | 214 GPa Show Material materials with Elastic modulus of 214 GPa | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
100 °C | 207 - 209 GPa Show Material materials with Elastic modulus of 207 - 209 GPa | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
100 °C | 207 GPa Show Material materials with Elastic modulus of 207 GPa | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
100 °C | 207 - 207.5 GPa Show Material materials with Elastic modulus of 207 - 207.5 GPa | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
100 °C | 207.5 - 209 GPa Show Material materials with Elastic modulus of 207.5 - 209 GPa | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
100 °C | 207.5 GPa Show Material materials with Elastic modulus of 207.5 GPa | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
100 °C | 209 GPa Show Material materials with Elastic modulus of 209 GPa | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
200 °C | 199 - 202 GPa Show Material materials with Elastic modulus of 199 - 202 GPa | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
200 °C | 199 GPa Show Material materials with Elastic modulus of 199 GPa | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
200 °C | 199 - 201.2 GPa Show Material materials with Elastic modulus of 199 - 201.2 GPa | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
200 °C | 201.2 - 202 GPa Show Material materials with Elastic modulus of 201.2 - 202 GPa | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
200 °C | 201.2 GPa Show Material materials with Elastic modulus of 201.2 GPa | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
200 °C | 202 GPa Show Material materials with Elastic modulus of 202 GPa | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
300 °C | 192 - 195 GPa Show Material materials with Elastic modulus of 192 - 195 GPa | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
300 °C | 192 GPa Show Material materials with Elastic modulus of 192 GPa | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
300 °C | 192 - 193.9 GPa Show Material materials with Elastic modulus of 192 - 193.9 GPa | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
300 °C | 193.9 - 195 GPa Show Material materials with Elastic modulus of 193.9 - 195 GPa | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
300 °C | 193.9 GPa Show Material materials with Elastic modulus of 193.9 GPa | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
300 °C | 195 GPa Show Material materials with Elastic modulus of 195 GPa | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
400 °C | 184 - 187 GPa Show Material materials with Elastic modulus of 184 - 187 GPa | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
400 °C | 184 GPa Show Material materials with Elastic modulus of 184 GPa | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
400 °C | 184 - 185.2 GPa Show Material materials with Elastic modulus of 184 - 185.2 GPa | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
400 °C | 185.2 - 187 GPa Show Material materials with Elastic modulus of 185.2 - 187 GPa | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
400 °C | 185.2 GPa Show Material materials with Elastic modulus of 185.2 GPa | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
400 °C | 187 GPa Show Material materials with Elastic modulus of 187 GPa | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
500 °C | 174.9 - 177 GPa Show Material materials with Elastic modulus of 174.9 - 177 GPa | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
500 °C | 174.9 - 175 GPa Show Material materials with Elastic modulus of 174.9 - 175 GPa | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
500 °C | 174.9 GPa Show Material materials with Elastic modulus of 174.9 GPa | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
500 °C | 175 - 177 GPa Show Material materials with Elastic modulus of 175 - 177 GPa | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
500 °C | 175 GPa Show Material materials with Elastic modulus of 175 GPa | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
500 °C | 177 GPa Show Material materials with Elastic modulus of 177 GPa | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
600 °C | 163.2 - 167 GPa Show Material materials with Elastic modulus of 163.2 - 167 GPa | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
600 °C | 163.2 - 164 GPa Show Material materials with Elastic modulus of 163.2 - 164 GPa | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
600 °C | 163.2 GPa Show Material materials with Elastic modulus of 163.2 GPa | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
600 °C | 164 - 167 GPa Show Material materials with Elastic modulus of 164 - 167 GPa | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
600 °C | 164 GPa Show Material materials with Elastic modulus of 164 GPa | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
600 °C | 167 GPa Show Material materials with Elastic modulus of 167 GPa | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
Elongation | 16.2 % Show Material materials with Elongation of 16.2 % | Predicted Value, A80 | ||||
16.4 % Show Material materials with Elongation of 16.4 % | Predicted Value, A80 Transverse | |||||
17.8 % Show Material materials with Elongation of 17.8 % | Predicted Value, A200 | |||||
20.5 % Show Material materials with Elongation of 20.5 % | Predicted Value, A5 | |||||
22 % Show Material materials with Elongation of 22 % | Predicted Value, A50 | |||||
20 °C | 17 % Show Material materials with Elongation of 17 % | normalized and tempered (+NT) | EN 10028-2 | Flat | Transverse | |
20 °C | 17 % Show Material materials with Elongation of 17 % | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
20 °C | 18 % Show Material materials with Elongation of 18 % | normalized and tempered (+NT) | EN 10028-2 | Flat | Transverse | |
20 °C | 18 % Show Material materials with Elongation of 18 % | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
Hardness, Brinell | 227 [-] Show Material materials with Hardness, Brinell of 227 [-] | Predicted Value, Transverse | ||||
Poisson's ratio | 20 °C | 0.283 [-] Show Material materials with Poisson's ratio of 0.283 [-] | normalized and tempered (+NT) | EN 10028-2 | Flat | |
100 °C | 0.286 [-] Show Material materials with Poisson's ratio of 0.286 [-] | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
200 °C | 0.292 [-] Show Material materials with Poisson's ratio of 0.292 [-] | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
300 °C | 0.294 [-] Show Material materials with Poisson's ratio of 0.294 [-] | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
400 °C | 0.3 [-] Show Material materials with Poisson's ratio of 0.3 [-] | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
500 °C | 0.307 [-] Show Material materials with Poisson's ratio of 0.307 [-] | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
600 °C | 0.313 [-] Show Material materials with Poisson's ratio of 0.313 [-] | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
Reduction of area | 42.1 % Show Material materials with Reduction of area of 42.1 % | Predicted Value | ||||
45.7 % Show Material materials with Reduction of area of 45.7 % | Predicted Value, Transverse | |||||
Shear modulus | 20 °C | 82.8 GPa Show Material materials with Shear modulus of 82.8 GPa | normalized and tempered (+NT) | EN 10028-2 | Flat | |
100 °C | 80.7 GPa Show Material materials with Shear modulus of 80.7 GPa | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
200 °C | 77.9 GPa Show Material materials with Shear modulus of 77.9 GPa | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
300 °C | 74.9 GPa Show Material materials with Shear modulus of 74.9 GPa | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
400 °C | 71.2 GPa Show Material materials with Shear modulus of 71.2 GPa | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
500 °C | 66.9 GPa Show Material materials with Shear modulus of 66.9 GPa | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
600 °C | 62.1 GPa Show Material materials with Shear modulus of 62.1 GPa | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
Shear strength | 604 MPa Show Material materials with Shear strength of 604 MPa | Predicted Value | ||||
Tensile strength | 20 °C | 470 - 630 MPa Show Material materials with Tensile strength of 470 - 630 MPa | normalized and tempered (+NT) | EN 10028-2 | Flat | Transverse |
20 °C | 470 - 620 MPa Show Material materials with Tensile strength of 470 - 620 MPa | normalized and tempered (+NT) | EN 10028-2 | Flat | Transverse | |
20 °C | 470 - 630 MPa Show Material materials with Tensile strength of 470 - 630 MPa | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
20 °C | 470 - 620 MPa Show Material materials with Tensile strength of 470 - 620 MPa | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
20 °C | 480 - 630 MPa Show Material materials with Tensile strength of 480 - 630 MPa | normalized and tempered (+NT) | EN 10028-2 | Flat | Transverse | |
20 °C | 480 - 620 MPa Show Material materials with Tensile strength of 480 - 620 MPa | normalized and tempered (+NT) | EN 10028-2 | Flat | Transverse | |
20 °C | 480 - 630 MPa Show Material materials with Tensile strength of 480 - 630 MPa | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
20 °C | 480 - 620 MPa Show Material materials with Tensile strength of 480 - 620 MPa | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
Yield strength | 260.9 MPa Show Material materials with Yield strength of 260.9 MPa | Predicted Value, RP1 | ||||
266.1 MPa Show Material materials with Yield strength of 266.1 MPa | Predicted Value, RP1 Transverse | |||||
380.7 MPa Show Material materials with Yield strength of 380.7 MPa | Predicted Value, RP05 | |||||
382 MPa Show Material materials with Yield strength of 382 MPa | Predicted Value, RP02 Transverse | |||||
485.8 MPa Show Material materials with Yield strength of 485.8 MPa | Predicted Value, RP002 | |||||
20 °C | 280 MPa Show Material materials with Yield strength of 280 MPa | normalized and tempered (+NT) | EN 10028-2 | Flat | Transverse | |
20 °C | 280 MPa Show Material materials with Yield strength of 280 MPa | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
20 °C | 290 MPa Show Material materials with Yield strength of 290 MPa | normalized and tempered (+NT) | EN 10028-2 | Flat | Transverse | |
20 °C | 290 MPa Show Material materials with Yield strength of 290 MPa | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
20 °C | 300 MPa Show Material materials with Yield strength of 300 MPa | normalized and tempered (+NT) | EN 10028-2 | Flat | Transverse | |
20 °C | 300 MPa Show Material materials with Yield strength of 300 MPa | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
20 °C | 310 MPa Show Material materials with Yield strength of 310 MPa | normalized and tempered (+NT) | EN 10028-2 | Flat | Transverse | |
20 °C | 310 MPa Show Material materials with Yield strength of 310 MPa | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
50 °C | 260 MPa Show Material materials with Yield strength of 260 MPa | normalized and tempered (+NT) | EN 10028-2 | Flat | RP02 | |
50 °C | 270 MPa Show Material materials with Yield strength of 270 MPa | normalized and tempered (+NT) | EN 10028-2 | Flat | RP02 | |
50 °C | 279 MPa Show Material materials with Yield strength of 279 MPa | normalized and tempered (+NT) | EN 10028-2 | Flat | RP02 | |
50 °C | 288 MPa Show Material materials with Yield strength of 288 MPa | normalized and tempered (+NT) | EN 10028-2 | Flat | RP02 | |
100 °C | 240 MPa Show Material materials with Yield strength of 240 MPa | normalized and tempered (+NT) | EN 10028-2 | Flat | RP02 | |
100 °C | 249 MPa Show Material materials with Yield strength of 249 MPa | normalized and tempered (+NT) | EN 10028-2 | Flat | RP02 | |
100 °C | 257 MPa Show Material materials with Yield strength of 257 MPa | normalized and tempered (+NT) | EN 10028-2 | Flat | RP02 | |
100 °C | 266 MPa Show Material materials with Yield strength of 266 MPa | normalized and tempered (+NT) | EN 10028-2 | Flat | RP02 | |
150 °C | 230 MPa Show Material materials with Yield strength of 230 MPa | normalized and tempered (+NT) | EN 10028-2 | Flat | RP02 | |
150 °C | 238 MPa Show Material materials with Yield strength of 238 MPa | normalized and tempered (+NT) | EN 10028-2 | Flat | RP02 | |
150 °C | 246 MPa Show Material materials with Yield strength of 246 MPa | normalized and tempered (+NT) | EN 10028-2 | Flat | RP02 | |
150 °C | 254 MPa Show Material materials with Yield strength of 254 MPa | normalized and tempered (+NT) | EN 10028-2 | Flat | RP02 | |
200 °C | 224 MPa Show Material materials with Yield strength of 224 MPa | normalized and tempered (+NT) | EN 10028-2 | Flat | RP02 | |
200 °C | 232 MPa Show Material materials with Yield strength of 232 MPa | normalized and tempered (+NT) | EN 10028-2 | Flat | RP02 | |
200 °C | 240 MPa Show Material materials with Yield strength of 240 MPa | normalized and tempered (+NT) | EN 10028-2 | Flat | RP02 | |
200 °C | 248 MPa Show Material materials with Yield strength of 248 MPa | normalized and tempered (+NT) | EN 10028-2 | Flat | RP02 | |
250 °C | 220 MPa Show Material materials with Yield strength of 220 MPa | normalized and tempered (+NT) | EN 10028-2 | Flat | RP02 | |
250 °C | 227 MPa Show Material materials with Yield strength of 227 MPa | normalized and tempered (+NT) | EN 10028-2 | Flat | RP02 | |
250 °C | 235 MPa Show Material materials with Yield strength of 235 MPa | normalized and tempered (+NT) | EN 10028-2 | Flat | RP02 | |
250 °C | 243 MPa Show Material materials with Yield strength of 243 MPa | normalized and tempered (+NT) | EN 10028-2 | Flat | RP02 | |
300 °C | 213 MPa Show Material materials with Yield strength of 213 MPa | normalized and tempered (+NT) | EN 10028-2 | Flat | RP02 | |
300 °C | 221 MPa Show Material materials with Yield strength of 221 MPa | normalized and tempered (+NT) | EN 10028-2 | Flat | RP02 | |
300 °C | 228 MPa Show Material materials with Yield strength of 228 MPa | normalized and tempered (+NT) | EN 10028-2 | Flat | RP02 | |
300 °C | 236 MPa Show Material materials with Yield strength of 236 MPa | normalized and tempered (+NT) | EN 10028-2 | Flat | RP02 | |
350 °C | 204 MPa Show Material materials with Yield strength of 204 MPa | normalized and tempered (+NT) | EN 10028-2 | Flat | RP02 | |
350 °C | 211 MPa Show Material materials with Yield strength of 211 MPa | normalized and tempered (+NT) | EN 10028-2 | Flat | RP02 | |
350 °C | 218 MPa Show Material materials with Yield strength of 218 MPa | normalized and tempered (+NT) | EN 10028-2 | Flat | RP02 | |
350 °C | 225 MPa Show Material materials with Yield strength of 225 MPa | normalized and tempered (+NT) | EN 10028-2 | Flat | RP02 | |
400 °C | 191 MPa Show Material materials with Yield strength of 191 MPa | normalized and tempered (+NT) | EN 10028-2 | Flat | RP02 | |
400 °C | 198 MPa Show Material materials with Yield strength of 198 MPa | normalized and tempered (+NT) | EN 10028-2 | Flat | RP02 | |
400 °C | 205 MPa Show Material materials with Yield strength of 205 MPa | normalized and tempered (+NT) | EN 10028-2 | Flat | RP02 | |
400 °C | 212 MPa Show Material materials with Yield strength of 212 MPa | normalized and tempered (+NT) | EN 10028-2 | Flat | RP02 | |
450 °C | 178 MPa Show Material materials with Yield strength of 178 MPa | normalized and tempered (+NT) | EN 10028-2 | Flat | RP02 | |
450 °C | 185 MPa Show Material materials with Yield strength of 185 MPa | normalized and tempered (+NT) | EN 10028-2 | Flat | RP02 | |
450 °C | 191 MPa Show Material materials with Yield strength of 191 MPa | normalized and tempered (+NT) | EN 10028-2 | Flat | RP02 | |
450 °C | 197 MPa Show Material materials with Yield strength of 197 MPa | normalized and tempered (+NT) | EN 10028-2 | Flat | RP02 | |
500 °C | 167 MPa Show Material materials with Yield strength of 167 MPa | normalized and tempered (+NT) | EN 10028-2 | Flat | RP02 | |
500 °C | 173 MPa Show Material materials with Yield strength of 173 MPa | normalized and tempered (+NT) | EN 10028-2 | Flat | RP02 | |
500 °C | 179 MPa Show Material materials with Yield strength of 179 MPa | normalized and tempered (+NT) | EN 10028-2 | Flat | RP02 | |
500 °C | 185 MPa Show Material materials with Yield strength of 185 MPa | normalized and tempered (+NT) | EN 10028-2 | Flat | RP02 |
Thermal
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Coefficient of thermal expansion | -100 °C | 1.05e-05 1/K Show Material materials with Coefficient of thermal expansion of 1.05e-05 1/K | normalized and tempered (+NT) | EN 10028-2 | Flat | |
20 °C | 1.15e-05 1/K Show Material materials with Coefficient of thermal expansion of 1.15e-05 1/K | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
100 °C | 1.21e-05 - 1.22e-05 1/K Show Material materials with Coefficient of thermal expansion of 1.21e-05 - 1.22e-05 1/K | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
100 °C | 1.21e-05 1/K Show Material materials with Coefficient of thermal expansion of 1.21e-05 1/K | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
100 °C | 1.22e-05 1/K Show Material materials with Coefficient of thermal expansion of 1.22e-05 1/K | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
200 °C | 1.27e-05 - 1.29e-05 1/K Show Material materials with Coefficient of thermal expansion of 1.27e-05 - 1.29e-05 1/K | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
200 °C | 1.27e-05 1/K Show Material materials with Coefficient of thermal expansion of 1.27e-05 1/K | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
200 °C | 1.29e-05 1/K Show Material materials with Coefficient of thermal expansion of 1.29e-05 1/K | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
300 °C | 1.32e-05 - 1.34e-05 1/K Show Material materials with Coefficient of thermal expansion of 1.32e-05 - 1.34e-05 1/K | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
300 °C | 1.32e-05 1/K Show Material materials with Coefficient of thermal expansion of 1.32e-05 1/K | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
300 °C | 1.34e-05 1/K Show Material materials with Coefficient of thermal expansion of 1.34e-05 1/K | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
400 °C | 1.36e-05 - 1.4e-05 1/K Show Material materials with Coefficient of thermal expansion of 1.36e-05 - 1.4e-05 1/K | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
400 °C | 1.36e-05 1/K Show Material materials with Coefficient of thermal expansion of 1.36e-05 1/K | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
400 °C | 1.4e-05 1/K Show Material materials with Coefficient of thermal expansion of 1.4e-05 1/K | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
500 °C | 1.4e-05 1/K Show Material materials with Coefficient of thermal expansion of 1.4e-05 1/K | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
500 °C | 1.4e-05 - 1.43e-05 1/K Show Material materials with Coefficient of thermal expansion of 1.4e-05 - 1.43e-05 1/K | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
500 °C | 1.43e-05 1/K Show Material materials with Coefficient of thermal expansion of 1.43e-05 1/K | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
600 °C | 1.44e-05 - 1.46e-05 1/K Show Material materials with Coefficient of thermal expansion of 1.44e-05 - 1.46e-05 1/K | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
600 °C | 1.44e-05 1/K Show Material materials with Coefficient of thermal expansion of 1.44e-05 1/K | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
600 °C | 1.46e-05 1/K Show Material materials with Coefficient of thermal expansion of 1.46e-05 1/K | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
Max service temperature | 400 - 550 °C Show Material materials with Max service temperature of 400 - 550 °C | normalized and tempered (+NT) | EN 10028-2 | Flat | Long | |
Melting point | 1382 - 1529 °C Show Material materials with Melting point of 1382 - 1529 °C | Typical for Chromium Molybdenum Steel | ||||
Specific heat capacity | -100 °C | 423 J/(kg·K) Show Material materials with Specific heat capacity of 423 J/(kg·K) | normalized and tempered (+NT) | EN 10028-2 | Flat | |
20 °C | 430 J/(kg·K) Show Material materials with Specific heat capacity of 430 J/(kg·K) | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
20 °C | 430 - 461 J/(kg·K) Show Material materials with Specific heat capacity of 430 - 461 J/(kg·K) | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
20 °C | 461 J/(kg·K) Show Material materials with Specific heat capacity of 461 J/(kg·K) | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
100 °C | 479 - 500 J/(kg·K) Show Material materials with Specific heat capacity of 479 - 500 J/(kg·K) | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
100 °C | 479 J/(kg·K) Show Material materials with Specific heat capacity of 479 J/(kg·K) | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
100 °C | 500 J/(kg·K) Show Material materials with Specific heat capacity of 500 J/(kg·K) | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
200 °C | 499 - 540 J/(kg·K) Show Material materials with Specific heat capacity of 499 - 540 J/(kg·K) | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
200 °C | 499 J/(kg·K) Show Material materials with Specific heat capacity of 499 J/(kg·K) | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
200 °C | 540 J/(kg·K) Show Material materials with Specific heat capacity of 540 J/(kg·K) | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
300 °C | 517 - 580 J/(kg·K) Show Material materials with Specific heat capacity of 517 - 580 J/(kg·K) | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
300 °C | 517 J/(kg·K) Show Material materials with Specific heat capacity of 517 J/(kg·K) | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
300 °C | 580 J/(kg·K) Show Material materials with Specific heat capacity of 580 J/(kg·K) | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
400 °C | 536 - 620 J/(kg·K) Show Material materials with Specific heat capacity of 536 - 620 J/(kg·K) | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
400 °C | 536 J/(kg·K) Show Material materials with Specific heat capacity of 536 J/(kg·K) | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
400 °C | 620 J/(kg·K) Show Material materials with Specific heat capacity of 620 J/(kg·K) | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
500 °C | 558 - 690 J/(kg·K) Show Material materials with Specific heat capacity of 558 - 690 J/(kg·K) | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
500 °C | 558 J/(kg·K) Show Material materials with Specific heat capacity of 558 J/(kg·K) | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
500 °C | 690 J/(kg·K) Show Material materials with Specific heat capacity of 690 J/(kg·K) | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
600 °C | 587 - 780 J/(kg·K) Show Material materials with Specific heat capacity of 587 - 780 J/(kg·K) | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
600 °C | 587 J/(kg·K) Show Material materials with Specific heat capacity of 587 J/(kg·K) | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
600 °C | 780 J/(kg·K) Show Material materials with Specific heat capacity of 780 J/(kg·K) | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
Thermal conductivity | 20 °C | 34.9 - 35 W/(m·K) Show Material materials with Thermal conductivity of 34.9 - 35 W/(m·K) | normalized and tempered (+NT) | EN 10028-2 | Flat | |
20 °C | 34.9 W/(m·K) Show Material materials with Thermal conductivity of 34.9 W/(m·K) | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
20 °C | 35 W/(m·K) Show Material materials with Thermal conductivity of 35 W/(m·K) | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
100 °C | 37 W/(m·K) Show Material materials with Thermal conductivity of 37 W/(m·K) | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
100 °C | 37 - 37.3 W/(m·K) Show Material materials with Thermal conductivity of 37 - 37.3 W/(m·K) | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
100 °C | 37.3 W/(m·K) Show Material materials with Thermal conductivity of 37.3 W/(m·K) | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
200 °C | 38 W/(m·K) Show Material materials with Thermal conductivity of 38 W/(m·K) | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
200 °C | 38 - 38.2 W/(m·K) Show Material materials with Thermal conductivity of 38 - 38.2 W/(m·K) | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
200 °C | 38.2 W/(m·K) Show Material materials with Thermal conductivity of 38.2 W/(m·K) | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
300 °C | 37.8 - 38 W/(m·K) Show Material materials with Thermal conductivity of 37.8 - 38 W/(m·K) | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
300 °C | 37.8 W/(m·K) Show Material materials with Thermal conductivity of 37.8 W/(m·K) | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
300 °C | 38 W/(m·K) Show Material materials with Thermal conductivity of 38 W/(m·K) | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
400 °C | 36.6 - 37 W/(m·K) Show Material materials with Thermal conductivity of 36.6 - 37 W/(m·K) | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
400 °C | 36.6 W/(m·K) Show Material materials with Thermal conductivity of 36.6 W/(m·K) | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
400 °C | 37 W/(m·K) Show Material materials with Thermal conductivity of 37 W/(m·K) | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
500 °C | 35 W/(m·K) Show Material materials with Thermal conductivity of 35 W/(m·K) | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
500 °C | 35 - 35.2 W/(m·K) Show Material materials with Thermal conductivity of 35 - 35.2 W/(m·K) | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
500 °C | 35.2 W/(m·K) Show Material materials with Thermal conductivity of 35.2 W/(m·K) | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
600 °C | 33 W/(m·K) Show Material materials with Thermal conductivity of 33 W/(m·K) | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
600 °C | 33 - 33.6 W/(m·K) Show Material materials with Thermal conductivity of 33 - 33.6 W/(m·K) | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
600 °C | 33.6 W/(m·K) Show Material materials with Thermal conductivity of 33.6 W/(m·K) | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
Thermal diffusivity | 20 °C | 9.7 mm²/s Show Material materials with Thermal diffusivity of 9.7 mm²/s | normalized and tempered (+NT) | EN 10028-2 | Flat | |
100 °C | 9.6 mm²/s Show Material materials with Thermal diffusivity of 9.6 mm²/s | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
200 °C | 9.2 mm²/s Show Material materials with Thermal diffusivity of 9.2 mm²/s | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
300 °C | 8.5 mm²/s Show Material materials with Thermal diffusivity of 8.5 mm²/s | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
400 °C | 7.8 mm²/s Show Material materials with Thermal diffusivity of 7.8 mm²/s | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
500 °C | 6.8 mm²/s Show Material materials with Thermal diffusivity of 6.8 mm²/s | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
600 °C | 5.7 mm²/s Show Material materials with Thermal diffusivity of 5.7 mm²/s | normalized and tempered (+NT) | EN 10028-2 | Flat |
Electrical
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Electrical conductivity | 3 S/m Show Material materials with Electrical conductivity of 3 S/m | Predicted Value | ||||
Electrical resistivity | 20 °C | 2.98e-07 - 3e-07 Ω·m Show Material materials with Electrical resistivity of 2.98e-07 - 3e-07 Ω·m | normalized and tempered (+NT) | EN 10028-2 | Flat | |
20 °C | 2.98e-07 Ω·m Show Material materials with Electrical resistivity of 2.98e-07 Ω·m | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
20 °C | 3e-07 Ω·m Show Material materials with Electrical resistivity of 3e-07 Ω·m | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
100 °C | 3.4e-07 Ω·m Show Material materials with Electrical resistivity of 3.4e-07 Ω·m | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
100 °C | 3.4e-07 - 3.43e-07 Ω·m Show Material materials with Electrical resistivity of 3.4e-07 - 3.43e-07 Ω·m | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
100 °C | 3.43e-07 Ω·m Show Material materials with Electrical resistivity of 3.43e-07 Ω·m | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
200 °C | 4.1e-07 Ω·m Show Material materials with Electrical resistivity of 4.1e-07 Ω·m | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
200 °C | 4.1e-07 - 4.13e-07 Ω·m Show Material materials with Electrical resistivity of 4.1e-07 - 4.13e-07 Ω·m | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
200 °C | 4.13e-07 Ω·m Show Material materials with Electrical resistivity of 4.13e-07 Ω·m | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
300 °C | 4.97e-07 - 5e-07 Ω·m Show Material materials with Electrical resistivity of 4.97e-07 - 5e-07 Ω·m | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
300 °C | 4.97e-07 Ω·m Show Material materials with Electrical resistivity of 4.97e-07 Ω·m | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
300 °C | 5e-07 Ω·m Show Material materials with Electrical resistivity of 5e-07 Ω·m | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
400 °C | 5.9e-07 Ω·m Show Material materials with Electrical resistivity of 5.9e-07 Ω·m | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
400 °C | 5.9e-07 - 5.95e-07 Ω·m Show Material materials with Electrical resistivity of 5.9e-07 - 5.95e-07 Ω·m | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
400 °C | 5.95e-07 Ω·m Show Material materials with Electrical resistivity of 5.95e-07 Ω·m | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
500 °C | 7e-07 Ω·m Show Material materials with Electrical resistivity of 7e-07 Ω·m | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
500 °C | 7e-07 - 7.03e-07 Ω·m Show Material materials with Electrical resistivity of 7e-07 - 7.03e-07 Ω·m | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
500 °C | 7.03e-07 Ω·m Show Material materials with Electrical resistivity of 7.03e-07 Ω·m | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
600 °C | 8.2e-07 Ω·m Show Material materials with Electrical resistivity of 8.2e-07 Ω·m | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
600 °C | 8.2e-07 - 8.25e-07 Ω·m Show Material materials with Electrical resistivity of 8.2e-07 - 8.25e-07 Ω·m | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
600 °C | 8.25e-07 Ω·m Show Material materials with Electrical resistivity of 8.25e-07 Ω·m | normalized and tempered (+NT) | EN 10028-2 | Flat |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Carbon | 0.08 - 0.14 % Show Material materials with Carbon of 0.08 - 0.14 % | normalized and tempered (+NT) | EN 10028-2 | Flat |
Chromium | 2 - 2.5 % Show Material materials with Chromium of 2 - 2.5 % | normalized and tempered (+NT) | EN 10028-2 | Flat |
Copper | 0.3 % Show Material materials with Copper of 0.3 % | normalized and tempered (+NT) | EN 10028-2 | Flat |
Manganese | 0.4 - 0.8 % Show Material materials with Manganese of 0.4 - 0.8 % | normalized and tempered (+NT) | EN 10028-2 | Flat |
Molybdenum | 0.9 - 1.1 % Show Material materials with Molybdenum of 0.9 - 1.1 % | normalized and tempered (+NT) | EN 10028-2 | Flat |
Nitrogen | 0.012 % Show Material materials with Nitrogen of 0.012 % | normalized and tempered (+NT) | EN 10028-2 | Flat |
Phosphorus | 0.02 % Show Material materials with Phosphorus of 0.02 % | normalized and tempered (+NT) | EN 10028-2 | Flat |
Silicon | 0.5 % Show Material materials with Silicon of 0.5 % | normalized and tempered (+NT) | EN 10028-2 | Flat |
Sulfur | 0.01 % Show Material materials with Sulfur of 0.01 % | normalized and tempered (+NT) | EN 10028-2 | Flat |
Technological properties
Property | ||
---|---|---|
Supplier Disclaimer | The given information is a rough description and some properties can depend on various factors such as product thickness. Please contact the supplier or refer to the related norm or standard for further information. |
Do you have a technical question or need more information about this material?