EN 10028-2 Grade 10CrMo9-10 quenched and tempered (+QT)

Want to keep this datasheet? Save it now in your required format

Description

Heat-resistant steel for application in pressure vessel and steam boiler construction. Furthermore application for collectors as well as in apparatus engineering and in oil-processing industry. Max. application temp.: 530 °C

Related Standards

Equivalent Materials

This material data has been provided by WIAM.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValue

Density

20.0 °C

7.84 g/cm³

Show Material materials with Density of 7.84 g/cm³

Mechanical

PropertyTemperatureValue

Elastic modulus

-100.0 °C

217 GPa

Show Material materials with Elastic modulus of 217 GPa

20.0 °C

212 - 214 GPa

Show Material materials with Elastic modulus of 212 - 214 GPa

100.0 °C

207 - 209 GPa

Show Material materials with Elastic modulus of 207 - 209 GPa

200.0 °C

199 - 202 GPa

Show Material materials with Elastic modulus of 199 - 202 GPa

300.0 °C

192 - 195 GPa

Show Material materials with Elastic modulus of 192 - 195 GPa

400.0 °C

184 - 187 GPa

Show Material materials with Elastic modulus of 184 - 187 GPa

500.0 °C

174.89 - 177 GPa

Show Material materials with Elastic modulus of 174.89 - 177 GPa

600.0 °C

163.15 - 167 GPa

Show Material materials with Elastic modulus of 163.15 - 167 GPa

Elongation

20.0 °C

17 %

Show Material materials with Elongation of 17 %

Elongation, transverse

20.0 °C

17 - 18 %

Show Material materials with Elongation, transverse of 17 - 18 %

Poisson's ratio

20.0 °C

0.28 [-]

Show Material materials with Poisson's ratio of 0.28 [-]

100.0 °C

0.29 [-]

Show Material materials with Poisson's ratio of 0.29 [-]

200.0 °C

0.29 [-]

Show Material materials with Poisson's ratio of 0.29 [-]

300.0 °C

0.29 [-]

Show Material materials with Poisson's ratio of 0.29 [-]

400.0 °C

0.3 [-]

Show Material materials with Poisson's ratio of 0.3 [-]

500.0 °C

0.31 [-]

Show Material materials with Poisson's ratio of 0.31 [-]

600.0 °C

0.31 [-]

Show Material materials with Poisson's ratio of 0.31 [-]

Unlock all property charts

Shear modulus

20.0 °C

82.81 GPa

Show Material materials with Shear modulus of 82.81 GPa

100.0 °C

80.65 GPa

Show Material materials with Shear modulus of 80.65 GPa

200.0 °C

77.87 GPa

Show Material materials with Shear modulus of 77.87 GPa

300.0 °C

74.93 GPa

Show Material materials with Shear modulus of 74.93 GPa

400.0 °C

71.22 GPa

Show Material materials with Shear modulus of 71.22 GPa

500.0 °C

66.9 GPa

Show Material materials with Shear modulus of 66.9 GPa

600.0 °C

62.11 GPa

Show Material materials with Shear modulus of 62.11 GPa

Unlock all property charts

Tensile strength

20.0 °C

450 - 610 MPa

Show Material materials with Tensile strength of 450 - 610 MPa

Tensile strength, transverse

20.0 °C

450 - 630 MPa

Show Material materials with Tensile strength, transverse of 450 - 630 MPa

Yield strength

20.0 °C

250 - 260 MPa

Show Material materials with Yield strength of 250 - 260 MPa

Yield strength Rp0.2

50.0 °C

240 - 250 MPa

Show Material materials with Yield strength Rp0.2 of 240 - 250 MPa

100.0 °C

227 - 237 MPa

Show Material materials with Yield strength Rp0.2 of 227 - 237 MPa

150.0 °C

219 - 228 MPa

Show Material materials with Yield strength Rp0.2 of 219 - 228 MPa

200.0 °C

213 - 222 MPa

Show Material materials with Yield strength Rp0.2 of 213 - 222 MPa

250.0 °C

210 - 219 MPa

Show Material materials with Yield strength Rp0.2 of 210 - 219 MPa

300.0 °C

208 - 213 MPa

Show Material materials with Yield strength Rp0.2 of 208 - 213 MPa

350.0 °C

204 MPa

Show Material materials with Yield strength Rp0.2 of 204 MPa

400.0 °C

191 MPa

Show Material materials with Yield strength Rp0.2 of 191 MPa

450.0 °C

178 MPa

Show Material materials with Yield strength Rp0.2 of 178 MPa

500.0 °C

167 MPa

Show Material materials with Yield strength Rp0.2 of 167 MPa

Unlock all property charts

Yield strength, transverse

20.0 °C

250 - 290 MPa

Show Material materials with Yield strength, transverse of 250 - 290 MPa

Thermal

PropertyTemperatureValueComment

Coefficient of thermal expansion

-100.0 °C

1.05E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.05E-5 1/K

20.0 °C

1.15E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.15E-5 1/K

100.0 °C

1.21E-5 - 1.22E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.21E-5 - 1.22E-5 1/K

200.0 °C

1.27E-5 - 1.29E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.27E-5 - 1.29E-5 1/K

300.0 °C

1.32E-5 - 1.34E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.32E-5 - 1.34E-5 1/K

400.0 °C

1.36E-5 - 1.4E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.36E-5 - 1.4E-5 1/K

500.0 °C

1.4E-5 - 1.43E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.4E-5 - 1.43E-5 1/K

600.0 °C

1.44E-5 - 1.46E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.44E-5 - 1.46E-5 1/K

Unlock all property charts

Max service temperature, long

400 - 550 °C

Show Material materials with Max service temperature, long of 400 - 550 °C

Melting point

1382 - 1529 °C

Show Material materials with Melting point of 1382 - 1529 °C

Typical for Chromium Molybdenum Steel

Specific heat capacity

-100.0 °C

423 J/(kg·K)

Show Material materials with Specific heat capacity of 423 J/(kg·K)

20.0 °C

430 - 461 J/(kg·K)

Show Material materials with Specific heat capacity of 430 - 461 J/(kg·K)

100.0 °C

479 - 500 J/(kg·K)

Show Material materials with Specific heat capacity of 479 - 500 J/(kg·K)

200.0 °C

499 - 540 J/(kg·K)

Show Material materials with Specific heat capacity of 499 - 540 J/(kg·K)

300.0 °C

517 - 580 J/(kg·K)

Show Material materials with Specific heat capacity of 517 - 580 J/(kg·K)

400.0 °C

536 - 620 J/(kg·K)

Show Material materials with Specific heat capacity of 536 - 620 J/(kg·K)

500.0 °C

558 - 690 J/(kg·K)

Show Material materials with Specific heat capacity of 558 - 690 J/(kg·K)

600.0 °C

587 - 780 J/(kg·K)

Show Material materials with Specific heat capacity of 587 - 780 J/(kg·K)

Unlock all property charts

Thermal conductivity

20.0 °C

34.9 - 35 W/(m·K)

Show Material materials with Thermal conductivity of 34.9 - 35 W/(m·K)

100.0 °C

37 - 37.3 W/(m·K)

Show Material materials with Thermal conductivity of 37 - 37.3 W/(m·K)

200.0 °C

38 - 38.2 W/(m·K)

Show Material materials with Thermal conductivity of 38 - 38.2 W/(m·K)

300.0 °C

37.8 - 38 W/(m·K)

Show Material materials with Thermal conductivity of 37.8 - 38 W/(m·K)

400.0 °C

36.6 - 37 W/(m·K)

Show Material materials with Thermal conductivity of 36.6 - 37 W/(m·K)

500.0 °C

35 - 35.2 W/(m·K)

Show Material materials with Thermal conductivity of 35 - 35.2 W/(m·K)

600.0 °C

33 - 33.6 W/(m·K)

Show Material materials with Thermal conductivity of 33 - 33.6 W/(m·K)

Unlock all property charts

Thermal diffusivity

20.0 °C

9.7 mm²/s

Show Material materials with Thermal diffusivity of 9.7 mm²/s

100.0 °C

9.6 mm²/s

Show Material materials with Thermal diffusivity of 9.6 mm²/s

200.0 °C

9.2 mm²/s

Show Material materials with Thermal diffusivity of 9.2 mm²/s

300.0 °C

8.5 mm²/s

Show Material materials with Thermal diffusivity of 8.5 mm²/s

400.0 °C

7.8 mm²/s

Show Material materials with Thermal diffusivity of 7.8 mm²/s

500.0 °C

6.8 mm²/s

Show Material materials with Thermal diffusivity of 6.8 mm²/s

600.0 °C

5.7 mm²/s

Show Material materials with Thermal diffusivity of 5.7 mm²/s

Unlock all property charts

Electrical

PropertyTemperatureValue

Electrical resistivity

20.0 °C

2.98E-7 - 3E-7 Ω·m

Show Material materials with Electrical resistivity of 2.98E-7 - 3E-7 Ω·m

100.0 °C

3.4E-7 - 3.43E-7 Ω·m

Show Material materials with Electrical resistivity of 3.4E-7 - 3.43E-7 Ω·m

200.0 °C

4.1E-7 - 4.13E-7 Ω·m

Show Material materials with Electrical resistivity of 4.1E-7 - 4.13E-7 Ω·m

300.0 °C

4.97E-7 - 5E-7 Ω·m

Show Material materials with Electrical resistivity of 4.97E-7 - 5E-7 Ω·m

400.0 °C

5.9E-7 - 5.95E-7 Ω·m

Show Material materials with Electrical resistivity of 5.9E-7 - 5.95E-7 Ω·m

500.0 °C

7E-7 - 7.03E-7 Ω·m

Show Material materials with Electrical resistivity of 7E-7 - 7.03E-7 Ω·m

600.0 °C

8.2E-7 - 8.25E-7 Ω·m

Show Material materials with Electrical resistivity of 8.2E-7 - 8.25E-7 Ω·m

Unlock all property charts

Chemical properties

PropertyValue

Carbon

0.08 - 0.14 %

Show Material materials with Carbon of 0.08 - 0.14 %

Chromium

2 - 2.5 %

Show Material materials with Chromium of 2 - 2.5 %

Copper

0.3 %

Show Material materials with Copper of 0.3 %

Manganese

0.4 - 0.8 %

Show Material materials with Manganese of 0.4 - 0.8 %

Molybdenum

0.9 - 1.1 %

Show Material materials with Molybdenum of 0.9 - 1.1 %

Nitrogen

0.01 %

Show Material materials with Nitrogen of 0.01 %

Phosphorus

0.02 %

Show Material materials with Phosphorus of 0.02 %

Silicon

0.5 %

Show Material materials with Silicon of 0.5 %

Sulfur

0.01 %

Show Material materials with Sulfur of 0.01 %