General
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Density | 20 °C | 7.848 - 7.85 g/cm³ Show Material materials with Density of 7.848 - 7.85 g/cm³ | normalized or normalized formed (+N) | EN 10028-2 | Flat |
20 °C | 7.848 - 7.86 g/cm³ Show Material materials with Density of 7.848 - 7.86 g/cm³ | normalized or normalized formed (+N) | EN 10028-2 | Flat | |
20 °C | 7.848 g/cm³ Show Material materials with Density of 7.848 g/cm³ | normalized or normalized formed (+N) | EN 10028-2 | Flat | |
20 °C | 7.85 g/cm³ Show Material materials with Density of 7.85 g/cm³ | normalized or normalized formed (+N) | EN 10028-2 | Flat | |
20 °C | 7.85 - 7.86 g/cm³ Show Material materials with Density of 7.85 - 7.86 g/cm³ | normalized or normalized formed (+N) | EN 10028-2 | Flat | |
20 °C | 7.86 g/cm³ Show Material materials with Density of 7.86 g/cm³ | normalized or normalized formed (+N) | EN 10028-2 | Sheet, Flat | |
50 °C | 7.839 g/cm³ Show Material materials with Density of 7.839 g/cm³ | normalized or normalized formed (+N) | EN 10028-2 | Flat | |
100 °C | 7.824 g/cm³ Show Material materials with Density of 7.824 g/cm³ | normalized or normalized formed (+N) | EN 10028-2 | Flat | |
150 °C | 7.808 g/cm³ Show Material materials with Density of 7.808 g/cm³ | normalized or normalized formed (+N) | EN 10028-2 | Flat | |
200 °C | 7.792 g/cm³ Show Material materials with Density of 7.792 g/cm³ | normalized or normalized formed (+N) | EN 10028-2 | Flat | |
250 °C | 7.774 g/cm³ Show Material materials with Density of 7.774 g/cm³ | normalized or normalized formed (+N) | EN 10028-2 | Flat | |
300 °C | 7.756 g/cm³ Show Material materials with Density of 7.756 g/cm³ | normalized or normalized formed (+N) | EN 10028-2 | Flat | |
350 °C | 7.738 g/cm³ Show Material materials with Density of 7.738 g/cm³ | normalized or normalized formed (+N) | EN 10028-2 | Flat | |
400 °C | 7.72 g/cm³ Show Material materials with Density of 7.72 g/cm³ | normalized or normalized formed (+N) | EN 10028-2 | Flat | |
450 °C | 7.701 g/cm³ Show Material materials with Density of 7.701 g/cm³ | normalized or normalized formed (+N) | EN 10028-2 | Flat | |
500 °C | 7.682 g/cm³ Show Material materials with Density of 7.682 g/cm³ | normalized or normalized formed (+N) | EN 10028-2 | Flat | |
550 °C | 7.662 g/cm³ Show Material materials with Density of 7.662 g/cm³ | normalized or normalized formed (+N) | EN 10028-2 | Flat | |
600 °C | 7.643 g/cm³ Show Material materials with Density of 7.643 g/cm³ | normalized or normalized formed (+N) | EN 10028-2 | Flat |
Mechanical
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Elastic modulus | -100 °C | 217 GPa Show Material materials with Elastic modulus of 217 GPa | normalized or normalized formed (+N) | EN 10028-2 | Flat, Sheet | |
20 °C | 212 GPa Show Material materials with Elastic modulus of 212 GPa | normalized or normalized formed (+N) | EN 10028-2 | Flat, Sheet | ||
20 °C | 212 - 212.5 GPa Show Material materials with Elastic modulus of 212 - 212.5 GPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
20 °C | 212.5 GPa Show Material materials with Elastic modulus of 212.5 GPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
50 °C | 211.6 GPa Show Material materials with Elastic modulus of 211.6 GPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
100 °C | 207 - 208 GPa Show Material materials with Elastic modulus of 207 - 208 GPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
100 °C | 207 GPa Show Material materials with Elastic modulus of 207 GPa | normalized or normalized formed (+N) | EN 10028-2 | Flat, Sheet | ||
100 °C | 207 - 209.2 GPa Show Material materials with Elastic modulus of 207 - 209.2 GPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
100 °C | 208 GPa Show Material materials with Elastic modulus of 208 GPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
100 °C | 208 - 209.2 GPa Show Material materials with Elastic modulus of 208 - 209.2 GPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
100 °C | 209.2 GPa Show Material materials with Elastic modulus of 209.2 GPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
150 °C | 206.1 GPa Show Material materials with Elastic modulus of 206.1 GPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
200 °C | 199 - 201 GPa Show Material materials with Elastic modulus of 199 - 201 GPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
200 °C | 199 GPa Show Material materials with Elastic modulus of 199 GPa | normalized or normalized formed (+N) | EN 10028-2 | Flat, Sheet | ||
200 °C | 199 - 202.5 GPa Show Material materials with Elastic modulus of 199 - 202.5 GPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
200 °C | 201 GPa Show Material materials with Elastic modulus of 201 GPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
200 °C | 201 - 202.5 GPa Show Material materials with Elastic modulus of 201 - 202.5 GPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
200 °C | 202.5 GPa Show Material materials with Elastic modulus of 202.5 GPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
250 °C | 198.4 GPa Show Material materials with Elastic modulus of 198.4 GPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
300 °C | 192 - 193 GPa Show Material materials with Elastic modulus of 192 - 193 GPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
300 °C | 192 GPa Show Material materials with Elastic modulus of 192 GPa | normalized or normalized formed (+N) | EN 10028-2 | Flat, Sheet | ||
300 °C | 192 - 194.1 GPa Show Material materials with Elastic modulus of 192 - 194.1 GPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
300 °C | 193 GPa Show Material materials with Elastic modulus of 193 GPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
300 °C | 193 - 194.1 GPa Show Material materials with Elastic modulus of 193 - 194.1 GPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
300 °C | 194.1 GPa Show Material materials with Elastic modulus of 194.1 GPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
350 °C | 189.8 GPa Show Material materials with Elastic modulus of 189.8 GPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
400 °C | 184 - 185 GPa Show Material materials with Elastic modulus of 184 - 185 GPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
400 °C | 184 GPa Show Material materials with Elastic modulus of 184 GPa | normalized or normalized formed (+N) | EN 10028-2 | Flat, Sheet | ||
400 °C | 184 - 185.5 GPa Show Material materials with Elastic modulus of 184 - 185.5 GPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
400 °C | 185 GPa Show Material materials with Elastic modulus of 185 GPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
400 °C | 185 - 185.5 GPa Show Material materials with Elastic modulus of 185 - 185.5 GPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
400 °C | 185.5 GPa Show Material materials with Elastic modulus of 185.5 GPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
450 °C | 181.0 GPa Show Material materials with Elastic modulus of 181.0 GPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
500 °C | 175 - 176 GPa Show Material materials with Elastic modulus of 175 - 176 GPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
500 °C | 175 GPa Show Material materials with Elastic modulus of 175 GPa | normalized or normalized formed (+N) | EN 10028-2 | Flat, Sheet | ||
500 °C | 175 - 176.5 GPa Show Material materials with Elastic modulus of 175 - 176.5 GPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
500 °C | 176 GPa Show Material materials with Elastic modulus of 176 GPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
500 °C | 176 - 176.5 GPa Show Material materials with Elastic modulus of 176 - 176.5 GPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
500 °C | 176.5 GPa Show Material materials with Elastic modulus of 176.5 GPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
550 °C | 172.0 GPa Show Material materials with Elastic modulus of 172.0 GPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
600 °C | 164 - 166 GPa Show Material materials with Elastic modulus of 164 - 166 GPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
600 °C | 164 GPa Show Material materials with Elastic modulus of 164 GPa | normalized or normalized formed (+N) | EN 10028-2 | Flat, Sheet | ||
600 °C | 164 - 167.0 GPa Show Material materials with Elastic modulus of 164 - 167.0 GPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
600 °C | 166 GPa Show Material materials with Elastic modulus of 166 GPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
600 °C | 166 - 167.0 GPa Show Material materials with Elastic modulus of 166 - 167.0 GPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
600 °C | 167.0 GPa Show Material materials with Elastic modulus of 167.0 GPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
Elongation | 17.3 % Show Material materials with Elongation of 17.3 % | Predicted Value, A80 Transverse | ||||
17.8 % Show Material materials with Elongation of 17.8 % | Predicted Value, A80 | |||||
18.1 % Show Material materials with Elongation of 18.1 % | Predicted Value, A200 | |||||
19.9 % Show Material materials with Elongation of 19.9 % | Predicted Value, A5 | |||||
25.8 % Show Material materials with Elongation of 25.8 % | Predicted Value, A50 | |||||
20 °C | 22 % Show Material materials with Elongation of 22 % | normalized or normalized formed (+N) | EN 10028-2 | Flat, Sheet | Transverse | |
20 °C | 22 % Show Material materials with Elongation of 22 % | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
Hardness, Brinell | 234 [-] Show Material materials with Hardness, Brinell of 234 [-] | Predicted Value, Transverse | ||||
Poisson's ratio | 20 °C | 0.286 [-] Show Material materials with Poisson's ratio of 0.286 [-] | normalized or normalized formed (+N) | EN 10028-2 | Flat | |
50 °C | 0.287 [-] Show Material materials with Poisson's ratio of 0.287 [-] | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
100 °C | 0.288 [-] Show Material materials with Poisson's ratio of 0.288 [-] | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
150 °C | 0.289 [-] Show Material materials with Poisson's ratio of 0.289 [-] | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
200 °C | 0.29 [-] Show Material materials with Poisson's ratio of 0.29 [-] | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
250 °C | 0.291 [-] Show Material materials with Poisson's ratio of 0.291 [-] | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
300 °C | 0.293 [-] Show Material materials with Poisson's ratio of 0.293 [-] | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
350 °C | 0.293 [-] Show Material materials with Poisson's ratio of 0.293 [-] | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
400 °C | 0.295 [-] Show Material materials with Poisson's ratio of 0.295 [-] | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
450 °C | 0.297 [-] Show Material materials with Poisson's ratio of 0.297 [-] | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
500 °C | 0.298 [-] Show Material materials with Poisson's ratio of 0.298 [-] | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
550 °C | 0.298 [-] Show Material materials with Poisson's ratio of 0.298 [-] | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
600 °C | 0.297 [-] Show Material materials with Poisson's ratio of 0.297 [-] | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
Reduction of area | 43.3 % Show Material materials with Reduction of area of 43.3 % | Predicted Value | ||||
43.4 % Show Material materials with Reduction of area of 43.4 % | Predicted Value, Transverse | |||||
Shear modulus | 20 °C | 82.6 GPa Show Material materials with Shear modulus of 82.6 GPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | |
50 °C | 82.2 GPa Show Material materials with Shear modulus of 82.2 GPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
100 °C | 81.2 GPa Show Material materials with Shear modulus of 81.2 GPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
150 °C | 80.0 GPa Show Material materials with Shear modulus of 80.0 GPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
200 °C | 78.5 GPa Show Material materials with Shear modulus of 78.5 GPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
250 °C | 76.8 GPa Show Material materials with Shear modulus of 76.8 GPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
300 °C | 75.0 GPa Show Material materials with Shear modulus of 75.0 GPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
350 °C | 73.4 GPa Show Material materials with Shear modulus of 73.4 GPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
400 °C | 71.6 GPa Show Material materials with Shear modulus of 71.6 GPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
450 °C | 69.8 GPa Show Material materials with Shear modulus of 69.8 GPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
500 °C | 68.0 GPa Show Material materials with Shear modulus of 68.0 GPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
550 °C | 66.2 GPa Show Material materials with Shear modulus of 66.2 GPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
600 °C | 64.3 GPa Show Material materials with Shear modulus of 64.3 GPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
Shear strength | 593 MPa Show Material materials with Shear strength of 593 MPa | Predicted Value | ||||
Tensile strength | 20 °C | 410 - 590 MPa Show Material materials with Tensile strength of 410 - 590 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | Transverse |
20 °C | 410 - 580 MPa Show Material materials with Tensile strength of 410 - 580 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | Transverse | |
20 °C | 410 - 570 MPa Show Material materials with Tensile strength of 410 - 570 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | Transverse | |
20 °C | 410 - 590 MPa Show Material materials with Tensile strength of 410 - 590 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
20 °C | 410 - 580 MPa Show Material materials with Tensile strength of 410 - 580 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
20 °C | 410 - 570 MPa Show Material materials with Tensile strength of 410 - 570 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
20 °C | 420 - 590 MPa Show Material materials with Tensile strength of 420 - 590 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | Transverse | |
20 °C | 420 - 580 MPa Show Material materials with Tensile strength of 420 - 580 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | Transverse | |
20 °C | 420 - 570 MPa Show Material materials with Tensile strength of 420 - 570 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | Transverse | |
20 °C | 420 - 590 MPa Show Material materials with Tensile strength of 420 - 590 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
20 °C | 420 - 580 MPa Show Material materials with Tensile strength of 420 - 580 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
20 °C | 420 - 570 MPa Show Material materials with Tensile strength of 420 - 570 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
20 °C | 430 - 590 MPa Show Material materials with Tensile strength of 430 - 590 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | Transverse | |
20 °C | 430 - 580 MPa Show Material materials with Tensile strength of 430 - 580 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | Transverse | |
20 °C | 430 - 570 MPa Show Material materials with Tensile strength of 430 - 570 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | Transverse | |
20 °C | 430 - 590 MPa Show Material materials with Tensile strength of 430 - 590 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
20 °C | 430 - 580 MPa Show Material materials with Tensile strength of 430 - 580 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
20 °C | 430 - 570 MPa Show Material materials with Tensile strength of 430 - 570 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
20 °C | 440 - 590 MPa Show Material materials with Tensile strength of 440 - 590 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat, Sheet | Transverse | |
20 °C | 440 - 580 MPa Show Material materials with Tensile strength of 440 - 580 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | Transverse | |
20 °C | 440 - 570 MPa Show Material materials with Tensile strength of 440 - 570 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | Transverse | |
20 °C | 440 - 590 MPa Show Material materials with Tensile strength of 440 - 590 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
20 °C | 440 - 580 MPa Show Material materials with Tensile strength of 440 - 580 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
20 °C | 440 - 570 MPa Show Material materials with Tensile strength of 440 - 570 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
Yield strength | 253.1 MPa Show Material materials with Yield strength of 253.1 MPa | Predicted Value, RP1 | ||||
265.3 MPa Show Material materials with Yield strength of 265.3 MPa | Predicted Value, RP1 Transverse | |||||
336.8 MPa Show Material materials with Yield strength of 336.8 MPa | Predicted Value, RP05 | |||||
345.6 MPa Show Material materials with Yield strength of 345.6 MPa | Predicted Value, RP02 Transverse | |||||
475.7 MPa Show Material materials with Yield strength of 475.7 MPa | Predicted Value, RP002 | |||||
20 °C | 210 MPa Show Material materials with Yield strength of 210 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | Transverse | |
20 °C | 210 MPa Show Material materials with Yield strength of 210 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
20 °C | 220 MPa Show Material materials with Yield strength of 220 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | Transverse | |
20 °C | 220 MPa Show Material materials with Yield strength of 220 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
20 °C | 240 MPa Show Material materials with Yield strength of 240 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | Transverse | |
20 °C | 240 MPa Show Material materials with Yield strength of 240 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
20 °C | 260 MPa Show Material materials with Yield strength of 260 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | Transverse | |
20 °C | 260 MPa Show Material materials with Yield strength of 260 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
20 °C | 270 MPa Show Material materials with Yield strength of 270 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | Transverse | |
20 °C | 270 MPa Show Material materials with Yield strength of 270 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
20 °C | 275 MPa Show Material materials with Yield strength of 275 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat, Sheet | Transverse | |
20 °C | 275 MPa Show Material materials with Yield strength of 275 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
50 °C | 208 MPa Show Material materials with Yield strength of 208 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
50 °C | 218 MPa Show Material materials with Yield strength of 218 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
50 °C | 238 MPa Show Material materials with Yield strength of 238 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
50 °C | 258 MPa Show Material materials with Yield strength of 258 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
50 °C | 268 MPa Show Material materials with Yield strength of 268 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
50 °C | 273 MPa Show Material materials with Yield strength of 273 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat, Sheet | RP02 | |
100 °C | 202 MPa Show Material materials with Yield strength of 202 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
100 °C | 211 MPa Show Material materials with Yield strength of 211 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
100 °C | 230 MPa Show Material materials with Yield strength of 230 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
100 °C | 250 MPa Show Material materials with Yield strength of 250 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat, Sheet | RP02 | |
100 °C | 259 MPa Show Material materials with Yield strength of 259 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
100 °C | 264 MPa Show Material materials with Yield strength of 264 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat, Sheet | RP02 | |
150 °C | 191 MPa Show Material materials with Yield strength of 191 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
150 °C | 200 MPa Show Material materials with Yield strength of 200 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
150 °C | 218 MPa Show Material materials with Yield strength of 218 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
150 °C | 236 MPa Show Material materials with Yield strength of 236 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
150 °C | 245 MPa Show Material materials with Yield strength of 245 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
150 °C | 250 MPa Show Material materials with Yield strength of 250 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat, Sheet | RP02 | |
200 °C | 178 MPa Show Material materials with Yield strength of 178 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
200 °C | 186 MPa Show Material materials with Yield strength of 186 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
200 °C | 203 MPa Show Material materials with Yield strength of 203 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
200 °C | 220 MPa Show Material materials with Yield strength of 220 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
200 °C | 228 MPa Show Material materials with Yield strength of 228 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
200 °C | 233 MPa Show Material materials with Yield strength of 233 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat, Sheet | RP02 | |
250 °C | 164 MPa Show Material materials with Yield strength of 164 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
250 °C | 171 MPa Show Material materials with Yield strength of 171 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
250 °C | 186 MPa Show Material materials with Yield strength of 186 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
250 °C | 202 MPa Show Material materials with Yield strength of 202 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
250 °C | 209 MPa Show Material materials with Yield strength of 209 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
250 °C | 213 MPa Show Material materials with Yield strength of 213 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat, Sheet | RP02 | |
300 °C | 148 MPa Show Material materials with Yield strength of 148 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
300 °C | 155 MPa Show Material materials with Yield strength of 155 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
300 °C | 169 MPa Show Material materials with Yield strength of 169 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
300 °C | 183 MPa Show Material materials with Yield strength of 183 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
300 °C | 190 MPa Show Material materials with Yield strength of 190 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
300 °C | 194 MPa Show Material materials with Yield strength of 194 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat, Sheet | RP02 | |
350 °C | 134 MPa Show Material materials with Yield strength of 134 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
350 °C | 140 MPa Show Material materials with Yield strength of 140 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
350 °C | 153 MPa Show Material materials with Yield strength of 153 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
350 °C | 165 MPa Show Material materials with Yield strength of 165 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
350 °C | 172 MPa Show Material materials with Yield strength of 172 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
350 °C | 175 MPa Show Material materials with Yield strength of 175 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat, Sheet | RP02 | |
400 °C | 121 MPa Show Material materials with Yield strength of 121 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
400 °C | 127 MPa Show Material materials with Yield strength of 127 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
400 °C | 139 MPa Show Material materials with Yield strength of 139 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
400 °C | 150 MPa Show Material materials with Yield strength of 150 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
400 °C | 156 MPa Show Material materials with Yield strength of 156 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
400 °C | 159 MPa Show Material materials with Yield strength of 159 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat, Sheet | RP02 | |
450 °C | 113 MPa Show Material materials with Yield strength of 113 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
450 °C | 118 MPa Show Material materials with Yield strength of 118 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
450 °C | 129 MPa Show Material materials with Yield strength of 129 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
450 °C | 139 MPa Show Material materials with Yield strength of 139 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
450 °C | 145 MPa Show Material materials with Yield strength of 145 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
450 °C | 147 MPa Show Material materials with Yield strength of 147 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat, Sheet | RP02 | |
500 °C | 108 MPa Show Material materials with Yield strength of 108 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
500 °C | 113 MPa Show Material materials with Yield strength of 113 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
500 °C | 123 MPa Show Material materials with Yield strength of 123 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
500 °C | 134 MPa Show Material materials with Yield strength of 134 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
500 °C | 139 MPa Show Material materials with Yield strength of 139 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
500 °C | 141 MPa Show Material materials with Yield strength of 141 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 |
Thermal
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Coefficient of thermal expansion | -100 °C | 1.05e-05 1/K Show Material materials with Coefficient of thermal expansion of 1.05e-05 1/K | normalized or normalized formed (+N) | EN 10028-2 | Flat, Sheet | |
20 °C | 1.15e-05 1/K Show Material materials with Coefficient of thermal expansion of 1.15e-05 1/K | normalized or normalized formed (+N) | EN 10028-2 | Flat, Sheet | ||
100 °C | 1.21e-05 - 1.22e-05 1/K Show Material materials with Coefficient of thermal expansion of 1.21e-05 - 1.22e-05 1/K | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
100 °C | 1.21e-05 1/K Show Material materials with Coefficient of thermal expansion of 1.21e-05 1/K | normalized or normalized formed (+N) | EN 10028-2 | Flat, Sheet | ||
100 °C | 1.22e-05 1/K Show Material materials with Coefficient of thermal expansion of 1.22e-05 1/K | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
200 °C | 1.27e-05 - 1.29e-05 1/K Show Material materials with Coefficient of thermal expansion of 1.27e-05 - 1.29e-05 1/K | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
200 °C | 1.27e-05 1/K Show Material materials with Coefficient of thermal expansion of 1.27e-05 1/K | normalized or normalized formed (+N) | EN 10028-2 | Flat, Sheet | ||
200 °C | 1.29e-05 1/K Show Material materials with Coefficient of thermal expansion of 1.29e-05 1/K | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
300 °C | 1.32e-05 - 1.34e-05 1/K Show Material materials with Coefficient of thermal expansion of 1.32e-05 - 1.34e-05 1/K | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
300 °C | 1.32e-05 1/K Show Material materials with Coefficient of thermal expansion of 1.32e-05 1/K | normalized or normalized formed (+N) | EN 10028-2 | Flat, Sheet | ||
300 °C | 1.34e-05 1/K Show Material materials with Coefficient of thermal expansion of 1.34e-05 1/K | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
400 °C | 1.36e-05 - 1.4e-05 1/K Show Material materials with Coefficient of thermal expansion of 1.36e-05 - 1.4e-05 1/K | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
400 °C | 1.36e-05 1/K Show Material materials with Coefficient of thermal expansion of 1.36e-05 1/K | normalized or normalized formed (+N) | EN 10028-2 | Flat, Sheet | ||
400 °C | 1.4e-05 1/K Show Material materials with Coefficient of thermal expansion of 1.4e-05 1/K | normalized or normalized formed (+N) | EN 10028-2 | Flat, Sheet | ||
500 °C | 1.4e-05 1/K Show Material materials with Coefficient of thermal expansion of 1.4e-05 1/K | normalized or normalized formed (+N) | EN 10028-2 | Flat, Sheet | ||
500 °C | 1.4e-05 - 1.43e-05 1/K Show Material materials with Coefficient of thermal expansion of 1.4e-05 - 1.43e-05 1/K | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
500 °C | 1.43e-05 1/K Show Material materials with Coefficient of thermal expansion of 1.43e-05 1/K | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
600 °C | 1.44e-05 - 1.46e-05 1/K Show Material materials with Coefficient of thermal expansion of 1.44e-05 - 1.46e-05 1/K | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
600 °C | 1.44e-05 1/K Show Material materials with Coefficient of thermal expansion of 1.44e-05 1/K | normalized or normalized formed (+N) | EN 10028-2 | Flat, Sheet | ||
600 °C | 1.46e-05 1/K Show Material materials with Coefficient of thermal expansion of 1.46e-05 1/K | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
Melting point | 1382 - 1529 °C Show Material materials with Melting point of 1382 - 1529 °C | Typical for Molybdenum Steel | ||||
Specific heat capacity | -100 °C | 423 J/(kg·K) Show Material materials with Specific heat capacity of 423 J/(kg·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat, Sheet | |
20 °C | 430 J/(kg·K) Show Material materials with Specific heat capacity of 430 J/(kg·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
20 °C | 430 - 461 J/(kg·K) Show Material materials with Specific heat capacity of 430 - 461 J/(kg·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
20 °C | 461 J/(kg·K) Show Material materials with Specific heat capacity of 461 J/(kg·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat, Sheet | ||
100 °C | 479 - 500 J/(kg·K) Show Material materials with Specific heat capacity of 479 - 500 J/(kg·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
100 °C | 479 J/(kg·K) Show Material materials with Specific heat capacity of 479 J/(kg·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat, Sheet | ||
100 °C | 500 J/(kg·K) Show Material materials with Specific heat capacity of 500 J/(kg·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
200 °C | 499 - 540 J/(kg·K) Show Material materials with Specific heat capacity of 499 - 540 J/(kg·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
200 °C | 499 J/(kg·K) Show Material materials with Specific heat capacity of 499 J/(kg·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat, Sheet | ||
200 °C | 540 J/(kg·K) Show Material materials with Specific heat capacity of 540 J/(kg·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
300 °C | 517 - 530 J/(kg·K) Show Material materials with Specific heat capacity of 517 - 530 J/(kg·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
300 °C | 517 J/(kg·K) Show Material materials with Specific heat capacity of 517 J/(kg·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat, Sheet | ||
300 °C | 530 J/(kg·K) Show Material materials with Specific heat capacity of 530 J/(kg·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
400 °C | 536 - 620 J/(kg·K) Show Material materials with Specific heat capacity of 536 - 620 J/(kg·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
400 °C | 536 J/(kg·K) Show Material materials with Specific heat capacity of 536 J/(kg·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat, Sheet | ||
400 °C | 620 J/(kg·K) Show Material materials with Specific heat capacity of 620 J/(kg·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
500 °C | 558 - 690 J/(kg·K) Show Material materials with Specific heat capacity of 558 - 690 J/(kg·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
500 °C | 558 J/(kg·K) Show Material materials with Specific heat capacity of 558 J/(kg·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat, Sheet | ||
500 °C | 690 J/(kg·K) Show Material materials with Specific heat capacity of 690 J/(kg·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
600 °C | 587 - 780 J/(kg·K) Show Material materials with Specific heat capacity of 587 - 780 J/(kg·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
600 °C | 587 J/(kg·K) Show Material materials with Specific heat capacity of 587 J/(kg·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat, Sheet | ||
600 °C | 780 J/(kg·K) Show Material materials with Specific heat capacity of 780 J/(kg·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
Thermal conductivity | 20 °C | 51 W/(m·K) Show Material materials with Thermal conductivity of 51 W/(m·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat | |
20 °C | 51 - 52.1 W/(m·K) Show Material materials with Thermal conductivity of 51 - 52.1 W/(m·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
20 °C | 52.1 W/(m·K) Show Material materials with Thermal conductivity of 52.1 W/(m·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat, Sheet | ||
100 °C | 51 W/(m·K) Show Material materials with Thermal conductivity of 51 W/(m·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
100 °C | 51 - 51.2 W/(m·K) Show Material materials with Thermal conductivity of 51 - 51.2 W/(m·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
100 °C | 51.2 W/(m·K) Show Material materials with Thermal conductivity of 51.2 W/(m·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat, Sheet | ||
200 °C | 48.7 - 49 W/(m·K) Show Material materials with Thermal conductivity of 48.7 - 49 W/(m·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
200 °C | 48.7 W/(m·K) Show Material materials with Thermal conductivity of 48.7 W/(m·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat, Sheet | ||
200 °C | 49 W/(m·K) Show Material materials with Thermal conductivity of 49 W/(m·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
300 °C | 45 W/(m·K) Show Material materials with Thermal conductivity of 45 W/(m·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
300 °C | 45 - 45.5 W/(m·K) Show Material materials with Thermal conductivity of 45 - 45.5 W/(m·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
300 °C | 45.5 W/(m·K) Show Material materials with Thermal conductivity of 45.5 W/(m·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat, Sheet | ||
400 °C | 42 W/(m·K) Show Material materials with Thermal conductivity of 42 W/(m·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
400 °C | 42 - 42.3 W/(m·K) Show Material materials with Thermal conductivity of 42 - 42.3 W/(m·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
400 °C | 42.3 W/(m·K) Show Material materials with Thermal conductivity of 42.3 W/(m·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat, Sheet | ||
500 °C | 39 W/(m·K) Show Material materials with Thermal conductivity of 39 W/(m·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
500 °C | 39 - 39.1 W/(m·K) Show Material materials with Thermal conductivity of 39 - 39.1 W/(m·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
500 °C | 39.1 W/(m·K) Show Material materials with Thermal conductivity of 39.1 W/(m·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat, Sheet | ||
600 °C | 36 W/(m·K) Show Material materials with Thermal conductivity of 36 W/(m·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat, Sheet | ||
Thermal diffusivity | 20 °C | 14.4 mm²/s Show Material materials with Thermal diffusivity of 14.4 mm²/s | normalized or normalized formed (+N) | EN 10028-2 | Flat, Sheet | |
100 °C | 13.2 mm²/s Show Material materials with Thermal diffusivity of 13.2 mm²/s | normalized or normalized formed (+N) | EN 10028-2 | Flat, Sheet | ||
200 °C | 11.7 mm²/s Show Material materials with Thermal diffusivity of 11.7 mm²/s | normalized or normalized formed (+N) | EN 10028-2 | Flat, Sheet | ||
300 °C | 10.3 mm²/s Show Material materials with Thermal diffusivity of 10.3 mm²/s | normalized or normalized formed (+N) | EN 10028-2 | Flat, Sheet | ||
400 °C | 9 mm²/s Show Material materials with Thermal diffusivity of 9 mm²/s | normalized or normalized formed (+N) | EN 10028-2 | Flat, Sheet | ||
500 °C | 7.5 mm²/s Show Material materials with Thermal diffusivity of 7.5 mm²/s | normalized or normalized formed (+N) | EN 10028-2 | Flat, Sheet | ||
600 °C | 6 mm²/s Show Material materials with Thermal diffusivity of 6 mm²/s | normalized or normalized formed (+N) | EN 10028-2 | Flat, Sheet |
Electrical
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Electrical conductivity | 5 S/m Show Material materials with Electrical conductivity of 5 S/m | Predicted Value | ||||
Electrical resistivity | 20 °C | 2e-07 Ω·m Show Material materials with Electrical resistivity of 2e-07 Ω·m | normalized or normalized formed (+N) | EN 10028-2 | Flat, Sheet | |
20 °C | 2e-07 - 2.16e-07 Ω·m Show Material materials with Electrical resistivity of 2e-07 - 2.16e-07 Ω·m | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
20 °C | 2.16e-07 Ω·m Show Material materials with Electrical resistivity of 2.16e-07 Ω·m | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
50 °C | 2.37e-07 Ω·m Show Material materials with Electrical resistivity of 2.37e-07 Ω·m | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
100 °C | 2.5e-07 Ω·m Show Material materials with Electrical resistivity of 2.5e-07 Ω·m | normalized or normalized formed (+N) | EN 10028-2 | Flat, Sheet | ||
100 °C | 2.5e-07 - 2.68e-07 Ω·m Show Material materials with Electrical resistivity of 2.5e-07 - 2.68e-07 Ω·m | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
100 °C | 2.68e-07 Ω·m Show Material materials with Electrical resistivity of 2.68e-07 Ω·m | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
150 °C | 3.02e-07 Ω·m Show Material materials with Electrical resistivity of 3.02e-07 Ω·m | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
200 °C | 3.24e-07 - 3.3e-07 Ω·m Show Material materials with Electrical resistivity of 3.24e-07 - 3.3e-07 Ω·m | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
200 °C | 3.24e-07 Ω·m Show Material materials with Electrical resistivity of 3.24e-07 Ω·m | normalized or normalized formed (+N) | EN 10028-2 | Flat, Sheet | ||
200 °C | 3.24e-07 - 3.39e-07 Ω·m Show Material materials with Electrical resistivity of 3.24e-07 - 3.39e-07 Ω·m | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
200 °C | 3.3e-07 Ω·m Show Material materials with Electrical resistivity of 3.3e-07 Ω·m | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
200 °C | 3.3e-07 - 3.39e-07 Ω·m Show Material materials with Electrical resistivity of 3.3e-07 - 3.39e-07 Ω·m | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
200 °C | 3.39e-07 Ω·m Show Material materials with Electrical resistivity of 3.39e-07 Ω·m | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
250 °C | 3.8e-07 Ω·m Show Material materials with Electrical resistivity of 3.8e-07 Ω·m | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
300 °C | 4.1e-07 Ω·m Show Material materials with Electrical resistivity of 4.1e-07 Ω·m | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
300 °C | 4.1e-07 - 4.12e-07 Ω·m Show Material materials with Electrical resistivity of 4.1e-07 - 4.12e-07 Ω·m | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
300 °C | 4.1e-07 - 4.25e-07 Ω·m Show Material materials with Electrical resistivity of 4.1e-07 - 4.25e-07 Ω·m | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
300 °C | 4.12e-07 Ω·m Show Material materials with Electrical resistivity of 4.12e-07 Ω·m | normalized or normalized formed (+N) | EN 10028-2 | Flat, Sheet | ||
300 °C | 4.12e-07 - 4.25e-07 Ω·m Show Material materials with Electrical resistivity of 4.12e-07 - 4.25e-07 Ω·m | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
300 °C | 4.25e-07 Ω·m Show Material materials with Electrical resistivity of 4.25e-07 Ω·m | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
350 °C | 4.74e-07 Ω·m Show Material materials with Electrical resistivity of 4.74e-07 Ω·m | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
400 °C | 5.14e-07 - 5.2e-07 Ω·m Show Material materials with Electrical resistivity of 5.14e-07 - 5.2e-07 Ω·m | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
400 °C | 5.14e-07 Ω·m Show Material materials with Electrical resistivity of 5.14e-07 Ω·m | normalized or normalized formed (+N) | EN 10028-2 | Flat, Sheet | ||
400 °C | 5.14e-07 - 5.27e-07 Ω·m Show Material materials with Electrical resistivity of 5.14e-07 - 5.27e-07 Ω·m | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
400 °C | 5.2e-07 Ω·m Show Material materials with Electrical resistivity of 5.2e-07 Ω·m | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
400 °C | 5.2e-07 - 5.27e-07 Ω·m Show Material materials with Electrical resistivity of 5.2e-07 - 5.27e-07 Ω·m | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
400 °C | 5.27e-07 Ω·m Show Material materials with Electrical resistivity of 5.27e-07 Ω·m | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
450 °C | 5.83e-07 Ω·m Show Material materials with Electrical resistivity of 5.83e-07 Ω·m | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
500 °C | 6.33e-07 - 6.4e-07 Ω·m Show Material materials with Electrical resistivity of 6.33e-07 - 6.4e-07 Ω·m | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
500 °C | 6.33e-07 Ω·m Show Material materials with Electrical resistivity of 6.33e-07 Ω·m | normalized or normalized formed (+N) | EN 10028-2 | Flat, Sheet | ||
500 °C | 6.33e-07 - 6.42e-07 Ω·m Show Material materials with Electrical resistivity of 6.33e-07 - 6.42e-07 Ω·m | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
500 °C | 6.4e-07 Ω·m Show Material materials with Electrical resistivity of 6.4e-07 Ω·m | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
500 °C | 6.4e-07 - 6.42e-07 Ω·m Show Material materials with Electrical resistivity of 6.4e-07 - 6.42e-07 Ω·m | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
500 °C | 6.42e-07 Ω·m Show Material materials with Electrical resistivity of 6.42e-07 Ω·m | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
550 °C | 7.08e-07 Ω·m Show Material materials with Electrical resistivity of 7.08e-07 Ω·m | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
600 °C | 7.69e-07 - 7.8e-07 Ω·m Show Material materials with Electrical resistivity of 7.69e-07 - 7.8e-07 Ω·m | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
600 °C | 7.69e-07 Ω·m Show Material materials with Electrical resistivity of 7.69e-07 Ω·m | normalized or normalized formed (+N) | EN 10028-2 | Flat, Sheet | ||
600 °C | 7.69e-07 - 7.78e-07 Ω·m Show Material materials with Electrical resistivity of 7.69e-07 - 7.78e-07 Ω·m | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
600 °C | 7.78e-07 - 7.8e-07 Ω·m Show Material materials with Electrical resistivity of 7.78e-07 - 7.8e-07 Ω·m | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
600 °C | 7.78e-07 Ω·m Show Material materials with Electrical resistivity of 7.78e-07 Ω·m | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
600 °C | 7.8e-07 Ω·m Show Material materials with Electrical resistivity of 7.8e-07 Ω·m | normalized or normalized formed (+N) | EN 10028-2 | Flat |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Carbon | 0.12 - 0.2 % Show Material materials with Carbon of 0.12 - 0.2 % | normalized or normalized formed (+N) | EN 10028-2 | Flat, Sheet |
Chromium | 0.3 % Show Material materials with Chromium of 0.3 % | normalized or normalized formed (+N) | EN 10028-2 | Flat, Sheet |
Copper | 0.3 % Show Material materials with Copper of 0.3 % | normalized or normalized formed (+N) | EN 10028-2 | Flat, Sheet |
Manganese | 0.4 - 0.9 % Show Material materials with Manganese of 0.4 - 0.9 % | normalized or normalized formed (+N) | EN 10028-2 | Flat, Sheet |
Molybdenum | 0.25 - 0.35 % Show Material materials with Molybdenum of 0.25 - 0.35 % | normalized or normalized formed (+N) | EN 10028-2 | Flat, Sheet |
Nickel | 0.3 % Show Material materials with Nickel of 0.3 % | normalized or normalized formed (+N) | EN 10028-2 | Flat, Sheet |
Nitrogen | 0.012 % Show Material materials with Nitrogen of 0.012 % | normalized or normalized formed (+N) | EN 10028-2 | Flat, Sheet |
Phosphorus | 0.025 % Show Material materials with Phosphorus of 0.025 % | normalized or normalized formed (+N) | EN 10028-2 | Flat, Sheet |
Silicon | 0.35 % Show Material materials with Silicon of 0.35 % | normalized or normalized formed (+N) | EN 10028-2 | Flat, Sheet |
Sulfur | 0.01 % Show Material materials with Sulfur of 0.01 % | normalized or normalized formed (+N) | EN 10028-2 | Flat, Sheet |
Technological properties
Property | ||
---|---|---|
Supplier Disclaimer | The given information is a rough description and some properties can depend on various factors such as product thickness. Please contact the supplier or refer to the related norm or standard for further information. |
Do you have a technical question or need more information about this material?
Post it as a comment below and receive answers from engineers and other community members.