EN 10028-3 Grade P275NL1 normalized or normalized formed (+N)

View suppliers (9)
Want to keep this datasheet? Save it now in your required format

Description

Cryogenic weldable fine grain steel for pressure vessel construction.

Related Standards

Equivalent Materials

This material data has been provided by WIAM.

"Typical" values were obtained via a literature search. "Predicted" values were imputed via artificial intelligence technology. While we have placed significant efforts in ensuring data accuracy, "typical" and "predicted" data should be considered indicative and verified by appropriate material testing. Please do contact us if additional information on the the predicted data method is required.
All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValueConditionRelated StandardsShape

Density

20 °C

7.84 g/cm³

Show Material materials with Density of 7.84 g/cm³

normalized or normalized formed (+N)

EN 10028-3

Flat

20 °C

7.84 - 7.85 g/cm³

Show Material materials with Density of 7.84 - 7.85 g/cm³

normalized or normalized formed (+N)

EN 10028-3

Flat

20 °C

7.85 g/cm³

Show Material materials with Density of 7.85 g/cm³

normalized or normalized formed (+N)

EN 10028-3

Flat

Mechanical

PropertyTemperatureValueConditionRelated StandardsShapeComment

Elastic modulus

-100 °C

217 GPa

Show Material materials with Elastic modulus of 217 GPa

normalized or normalized formed (+N)

EN 10028-3

Flat

20 °C

212 GPa

Show Material materials with Elastic modulus of 212 GPa

normalized or normalized formed (+N)

EN 10028-3

Flat

100 °C

207 GPa

Show Material materials with Elastic modulus of 207 GPa

normalized or normalized formed (+N)

EN 10028-3

Flat

200 °C

199 GPa

Show Material materials with Elastic modulus of 199 GPa

normalized or normalized formed (+N)

EN 10028-3

Flat

300 °C

192 GPa

Show Material materials with Elastic modulus of 192 GPa

normalized or normalized formed (+N)

EN 10028-3

Flat

400 °C

184 GPa

Show Material materials with Elastic modulus of 184 GPa

normalized or normalized formed (+N)

EN 10028-3

Flat

500 °C

175 GPa

Show Material materials with Elastic modulus of 175 GPa

normalized or normalized formed (+N)

EN 10028-3

Flat

600 °C

164 GPa

Show Material materials with Elastic modulus of 164 GPa

normalized or normalized formed (+N)

EN 10028-3

Flat

Elongation

18.3 %

Show Material materials with Elongation of 18.3 %

Predicted Value, A80 Transverse

18.6 %

Show Material materials with Elongation of 18.6 %

Predicted Value, A200

19.8 %

Show Material materials with Elongation of 19.8 %

Predicted Value, A80

21.2 %

Show Material materials with Elongation of 21.2 %

Predicted Value, A5

22.4 %

Show Material materials with Elongation of 22.4 %

Predicted Value, Transverse

24.5 %

Show Material materials with Elongation of 24.5 %

Predicted Value, A50

20 °C

22 %

Show Material materials with Elongation of 22 %

normalized or normalized formed (+N)

EN 10028-3

Sheet, Flat

20 °C

23 %

Show Material materials with Elongation of 23 %

normalized or normalized formed (+N)

EN 10028-3

Flat

20 °C

24 %

Show Material materials with Elongation of 24 %

normalized or normalized formed (+N)

EN 10028-3

Flat

Hardness, Brinell

242 [-]

Show Material materials with Hardness, Brinell of 242 [-]

Predicted Value, Transverse

Poisson's ratio

0.29 [-]

Show Material materials with Poisson's ratio of 0.29 [-]

Typical for Low Carbon Steel

Reduction of area

41.3 %

Show Material materials with Reduction of area of 41.3 %

Predicted Value

42.5 %

Show Material materials with Reduction of area of 42.5 %

Predicted Value, Transverse

Shear modulus

82 GPa

Show Material materials with Shear modulus of 82 GPa

Typical for Low Carbon Steel

Shear strength

505.4 MPa

Show Material materials with Shear strength of 505.4 MPa

Predicted Value

Tensile strength

20 °C

340 - 470 MPa

Show Material materials with Tensile strength of 340 - 470 MPa

normalized or normalized formed (+N)

EN 10028-3

Sheet, Flat

20 °C

350 - 510 MPa

Show Material materials with Tensile strength of 350 - 510 MPa

normalized or normalized formed (+N)

EN 10028-3

Flat

20 °C

350 - 490 MPa

Show Material materials with Tensile strength of 350 - 490 MPa

normalized or normalized formed (+N)

EN 10028-3

Flat

20 °C

350 - 480 MPa

Show Material materials with Tensile strength of 350 - 480 MPa

normalized or normalized formed (+N)

EN 10028-3

Flat

20 °C

350 - 470 MPa

Show Material materials with Tensile strength of 350 - 470 MPa

normalized or normalized formed (+N)

EN 10028-3

Flat

20 °C

360 - 510 MPa

Show Material materials with Tensile strength of 360 - 510 MPa

normalized or normalized formed (+N)

EN 10028-3

Flat

20 °C

360 - 490 MPa

Show Material materials with Tensile strength of 360 - 490 MPa

normalized or normalized formed (+N)

EN 10028-3

Flat

20 °C

360 - 480 MPa

Show Material materials with Tensile strength of 360 - 480 MPa

normalized or normalized formed (+N)

EN 10028-3

Flat

20 °C

360 - 470 MPa

Show Material materials with Tensile strength of 360 - 470 MPa

normalized or normalized formed (+N)

EN 10028-3

Flat

20 °C

370 - 510 MPa

Show Material materials with Tensile strength of 370 - 510 MPa

normalized or normalized formed (+N)

EN 10028-3

Flat

20 °C

370 - 490 MPa

Show Material materials with Tensile strength of 370 - 490 MPa

normalized or normalized formed (+N)

EN 10028-3

Flat

20 °C

370 - 480 MPa

Show Material materials with Tensile strength of 370 - 480 MPa

normalized or normalized formed (+N)

EN 10028-3

Flat

20 °C

370 - 470 MPa

Show Material materials with Tensile strength of 370 - 470 MPa

normalized or normalized formed (+N)

EN 10028-3

Flat

20 °C

390 - 510 MPa

Show Material materials with Tensile strength of 390 - 510 MPa

normalized or normalized formed (+N)

EN 10028-3

Flat

20 °C

390 - 490 MPa

Show Material materials with Tensile strength of 390 - 490 MPa

normalized or normalized formed (+N)

EN 10028-3

Flat

20 °C

390 - 480 MPa

Show Material materials with Tensile strength of 390 - 480 MPa

normalized or normalized formed (+N)

EN 10028-3

Flat

20 °C

390 - 470 MPa

Show Material materials with Tensile strength of 390 - 470 MPa

normalized or normalized formed (+N)

EN 10028-3

Flat

Yield strength

258.3 MPa

Show Material materials with Yield strength of 258.3 MPa

Predicted Value, RP1

300 MPa

Show Material materials with Yield strength of 300 MPa

Predicted Value, RP1 Transverse

311.7 MPa

Show Material materials with Yield strength of 311.7 MPa

Predicted Value, RP02

326.7 MPa

Show Material materials with Yield strength of 326.7 MPa

Predicted Value, Transverse

394.6 MPa

Show Material materials with Yield strength of 394.6 MPa

Predicted Value, RP05

452.1 MPa

Show Material materials with Yield strength of 452.1 MPa

Predicted Value, RP02 Transverse

461.3 MPa

Show Material materials with Yield strength of 461.3 MPa

Predicted Value, RP002

20 °C

215 MPa

Show Material materials with Yield strength of 215 MPa

normalized or normalized formed (+N)

EN 10028-3

Sheet, Flat

20 °C

225 MPa

Show Material materials with Yield strength of 225 MPa

normalized or normalized formed (+N)

EN 10028-3

Flat

20 °C

235 MPa

Show Material materials with Yield strength of 235 MPa

normalized or normalized formed (+N)

EN 10028-3

Flat

20 °C

255 MPa

Show Material materials with Yield strength of 255 MPa

normalized or normalized formed (+N)

EN 10028-3

Flat

20 °C

265 MPa

Show Material materials with Yield strength of 265 MPa

normalized or normalized formed (+N)

EN 10028-3

Flat

20 °C

275 MPa

Show Material materials with Yield strength of 275 MPa

normalized or normalized formed (+N)

EN 10028-3

Flat

Thermal

PropertyTemperatureValueConditionRelated StandardsShapeComment

Coefficient of thermal expansion

-100 °C

1.08e-05 1/K

Show Material materials with Coefficient of thermal expansion of 1.08e-05 1/K

normalized or normalized formed (+N)

EN 10028-3

Flat

20 °C

1.19e-05 1/K

Show Material materials with Coefficient of thermal expansion of 1.19e-05 1/K

normalized or normalized formed (+N)

EN 10028-3

Flat

100 °C

1.25e-05 1/K

Show Material materials with Coefficient of thermal expansion of 1.25e-05 1/K

normalized or normalized formed (+N)

EN 10028-3

Flat

200 °C

1.3e-05 1/K

Show Material materials with Coefficient of thermal expansion of 1.3e-05 1/K

normalized or normalized formed (+N)

EN 10028-3

Flat

300 °C

1.36e-05 1/K

Show Material materials with Coefficient of thermal expansion of 1.36e-05 1/K

normalized or normalized formed (+N)

EN 10028-3

Flat

400 °C

1.41e-05 1/K

Show Material materials with Coefficient of thermal expansion of 1.41e-05 1/K

normalized or normalized formed (+N)

EN 10028-3

Flat

500 °C

1.45e-05 1/K

Show Material materials with Coefficient of thermal expansion of 1.45e-05 1/K

normalized or normalized formed (+N)

EN 10028-3

Flat

600 °C

1.49e-05 1/K

Show Material materials with Coefficient of thermal expansion of 1.49e-05 1/K

normalized or normalized formed (+N)

EN 10028-3

Flat

Max service temperature

-60 °C

Show Material materials with Max service temperature of -60 °C

normalized or normalized formed (+N)

EN 10028-3

Flat

Long

500 °C

Show Material materials with Max service temperature of 500 °C

Typical for Carbon Steel

Melting point

1480 - 1526 °C

Show Material materials with Melting point of 1480 - 1526 °C

Typical for Low Carbon Steel

Specific heat capacity

-100 °C

423 J/(kg·K)

Show Material materials with Specific heat capacity of 423 J/(kg·K)

normalized or normalized formed (+N)

EN 10028-3

Flat

20 °C

430 J/(kg·K)

Show Material materials with Specific heat capacity of 430 J/(kg·K)

normalized or normalized formed (+N)

EN 10028-3

Flat

20 °C

430 - 461 J/(kg·K)

Show Material materials with Specific heat capacity of 430 - 461 J/(kg·K)

normalized or normalized formed (+N)

EN 10028-3

Flat

20 °C

461 J/(kg·K)

Show Material materials with Specific heat capacity of 461 J/(kg·K)

normalized or normalized formed (+N)

EN 10028-3

Flat

100 °C

479 J/(kg·K)

Show Material materials with Specific heat capacity of 479 J/(kg·K)

normalized or normalized formed (+N)

EN 10028-3

Flat

200 °C

499 J/(kg·K)

Show Material materials with Specific heat capacity of 499 J/(kg·K)

normalized or normalized formed (+N)

EN 10028-3

Flat

300 °C

517 J/(kg·K)

Show Material materials with Specific heat capacity of 517 J/(kg·K)

normalized or normalized formed (+N)

EN 10028-3

Flat

400 °C

536 J/(kg·K)

Show Material materials with Specific heat capacity of 536 J/(kg·K)

normalized or normalized formed (+N)

EN 10028-3

Flat

500 °C

558 J/(kg·K)

Show Material materials with Specific heat capacity of 558 J/(kg·K)

normalized or normalized formed (+N)

EN 10028-3

Flat

600 °C

587 J/(kg·K)

Show Material materials with Specific heat capacity of 587 J/(kg·K)

normalized or normalized formed (+N)

EN 10028-3

Flat

Thermal conductivity

-100 °C

52.6 W/(m·K)

Show Material materials with Thermal conductivity of 52.6 W/(m·K)

normalized or normalized formed (+N)

EN 10028-3

Flat

20 °C

53.4 - 54 W/(m·K)

Show Material materials with Thermal conductivity of 53.4 - 54 W/(m·K)

normalized or normalized formed (+N)

EN 10028-3

Flat

20 °C

53.4 W/(m·K)

Show Material materials with Thermal conductivity of 53.4 W/(m·K)

normalized or normalized formed (+N)

EN 10028-3

Flat

20 °C

54 W/(m·K)

Show Material materials with Thermal conductivity of 54 W/(m·K)

normalized or normalized formed (+N)

EN 10028-3

Flat

100 °C

53.3 W/(m·K)

Show Material materials with Thermal conductivity of 53.3 W/(m·K)

normalized or normalized formed (+N)

EN 10028-3

Flat

200 °C

50.1 W/(m·K)

Show Material materials with Thermal conductivity of 50.1 W/(m·K)

normalized or normalized formed (+N)

EN 10028-3

Flat

300 °C

46.9 W/(m·K)

Show Material materials with Thermal conductivity of 46.9 W/(m·K)

normalized or normalized formed (+N)

EN 10028-3

Flat

400 °C

43.2 W/(m·K)

Show Material materials with Thermal conductivity of 43.2 W/(m·K)

normalized or normalized formed (+N)

EN 10028-3

Flat

500 °C

39.5 W/(m·K)

Show Material materials with Thermal conductivity of 39.5 W/(m·K)

normalized or normalized formed (+N)

EN 10028-3

Flat

600 °C

36.1 W/(m·K)

Show Material materials with Thermal conductivity of 36.1 W/(m·K)

normalized or normalized formed (+N)

EN 10028-3

Flat

Thermal diffusivity

-100 °C

18 mm²/s

Show Material materials with Thermal diffusivity of 18 mm²/s

normalized or normalized formed (+N)

EN 10028-3

Flat

20 °C

14.8 mm²/s

Show Material materials with Thermal diffusivity of 14.8 mm²/s

normalized or normalized formed (+N)

EN 10028-3

Flat

100 °C

13.7 mm²/s

Show Material materials with Thermal diffusivity of 13.7 mm²/s

normalized or normalized formed (+N)

EN 10028-3

Flat

200 °C

12.1 mm²/s

Show Material materials with Thermal diffusivity of 12.1 mm²/s

normalized or normalized formed (+N)

EN 10028-3

Flat

300 °C

10.6 mm²/s

Show Material materials with Thermal diffusivity of 10.6 mm²/s

normalized or normalized formed (+N)

EN 10028-3

Flat

400 °C

9.2 mm²/s

Show Material materials with Thermal diffusivity of 9.2 mm²/s

normalized or normalized formed (+N)

EN 10028-3

Flat

500 °C

7.6 mm²/s

Show Material materials with Thermal diffusivity of 7.6 mm²/s

normalized or normalized formed (+N)

EN 10028-3

Flat

600 °C

6.1 mm²/s

Show Material materials with Thermal diffusivity of 6.1 mm²/s

normalized or normalized formed (+N)

EN 10028-3

Flat

Electrical

PropertyTemperatureValueConditionRelated StandardsShapeComment

Electrical conductivity

5 S/m

Show Material materials with Electrical conductivity of 5 S/m

Predicted Value

Electrical resistivity

-100 °C

1.3e-07 Ω·m

Show Material materials with Electrical resistivity of 1.3e-07 Ω·m

normalized or normalized formed (+N)

EN 10028-3

Flat

20 °C

1.95e-07 - 2e-07 Ω·m

Show Material materials with Electrical resistivity of 1.95e-07 - 2e-07 Ω·m

normalized or normalized formed (+N)

EN 10028-3

Flat

20 °C

1.95e-07 Ω·m

Show Material materials with Electrical resistivity of 1.95e-07 Ω·m

normalized or normalized formed (+N)

EN 10028-3

Flat

20 °C

2e-07 Ω·m

Show Material materials with Electrical resistivity of 2e-07 Ω·m

normalized or normalized formed (+N)

EN 10028-3

Flat

100 °C

2.4e-07 Ω·m

Show Material materials with Electrical resistivity of 2.4e-07 Ω·m

normalized or normalized formed (+N)

EN 10028-3

Flat

200 °C

3.15e-07 Ω·m

Show Material materials with Electrical resistivity of 3.15e-07 Ω·m

normalized or normalized formed (+N)

EN 10028-3

Flat

300 °C

4e-07 Ω·m

Show Material materials with Electrical resistivity of 4e-07 Ω·m

normalized or normalized formed (+N)

EN 10028-3

Flat

400 °C

5.03e-07 Ω·m

Show Material materials with Electrical resistivity of 5.03e-07 Ω·m

normalized or normalized formed (+N)

EN 10028-3

Flat

500 °C

6.26e-07 Ω·m

Show Material materials with Electrical resistivity of 6.26e-07 Ω·m

normalized or normalized formed (+N)

EN 10028-3

Flat

600 °C

7.68e-07 Ω·m

Show Material materials with Electrical resistivity of 7.68e-07 Ω·m

normalized or normalized formed (+N)

EN 10028-3

Flat

Magnetic

PropertyValueComment

Curie temperature

770 °C

Show Material materials with Curie temperature of 770 °C

Typical for Low Carbon Steel

Chemical properties

PropertyValueConditionRelated StandardsShape

Aluminium

0.02 %

Show Material materials with Aluminium of 0.02 %

normalized or normalized formed (+N)

EN 10028-3

Flat, Sheet

Carbon

0.16 %

Show Material materials with Carbon of 0.16 %

normalized or normalized formed (+N)

EN 10028-3

Flat, Sheet

Chromium

0.3 %

Show Material materials with Chromium of 0.3 %

normalized or normalized formed (+N)

EN 10028-3

Flat, Sheet

Copper

0.3 %

Show Material materials with Copper of 0.3 %

normalized or normalized formed (+N)

EN 10028-3

Flat, Sheet

Manganese

0.8 - 1.5 %

Show Material materials with Manganese of 0.8 - 1.5 %

normalized or normalized formed (+N)

EN 10028-3

Flat, Sheet

Molybdenum

0.08 %

Show Material materials with Molybdenum of 0.08 %

normalized or normalized formed (+N)

EN 10028-3

Flat, Sheet

Nickel

0.5 %

Show Material materials with Nickel of 0.5 %

normalized or normalized formed (+N)

EN 10028-3

Flat, Sheet

Niobium

0.05 %

Show Material materials with Niobium of 0.05 %

normalized or normalized formed (+N)

EN 10028-3

Flat, Sheet

Nitrogen

0.012 %

Show Material materials with Nitrogen of 0.012 %

normalized or normalized formed (+N)

EN 10028-3

Flat, Sheet

Phosphorus

0.025 %

Show Material materials with Phosphorus of 0.025 %

normalized or normalized formed (+N)

EN 10028-3

Flat, Sheet

Silicon

0.4 %

Show Material materials with Silicon of 0.4 %

normalized or normalized formed (+N)

EN 10028-3

Flat, Sheet

Sulfur

0.015 %

Show Material materials with Sulfur of 0.015 %

normalized or normalized formed (+N)

EN 10028-3

Flat, Sheet

Titanium

0.03 %

Show Material materials with Titanium of 0.03 %

normalized or normalized formed (+N)

EN 10028-3

Flat, Sheet

Vanadium

0.05 %

Show Material materials with Vanadium of 0.05 %

normalized or normalized formed (+N)

EN 10028-3

Flat, Sheet

Technological properties

Property
Supplier Disclaimer

The given information is a rough description and some properties can depend on various factors such as product thickness. Please contact the supplier or refer to the related norm or standard for further information.