General
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Density | 20 °C | 7.83 - 7.84 g/cm³ Show Material materials with Density of 7.83 - 7.84 g/cm³ | normalized or normalized formed (+N) | EN 10028-3 | Flat |
20 °C | 7.83 g/cm³ Show Material materials with Density of 7.83 g/cm³ | normalized or normalized formed (+N) | EN 10028-3 | Flat | |
20 °C | 7.84 g/cm³ Show Material materials with Density of 7.84 g/cm³ | normalized or normalized formed (+N) | EN 10028-3 | Flat |
Mechanical
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Elastic modulus | -100 °C | 217 GPa Show Material materials with Elastic modulus of 217 GPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | |
20 °C | 212 GPa Show Material materials with Elastic modulus of 212 GPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
100 °C | 207 GPa Show Material materials with Elastic modulus of 207 GPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
200 °C | 199 GPa Show Material materials with Elastic modulus of 199 GPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
300 °C | 192 GPa Show Material materials with Elastic modulus of 192 GPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
400 °C | 184 GPa Show Material materials with Elastic modulus of 184 GPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
500 °C | 175 GPa Show Material materials with Elastic modulus of 175 GPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
600 °C | 164 GPa Show Material materials with Elastic modulus of 164 GPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
Elongation | 17.1 % Show Material materials with Elongation of 17.1 % | Predicted Value, A80 | ||||
17.2 % Show Material materials with Elongation of 17.2 % | Predicted Value, A80 Transverse | |||||
17.8 % Show Material materials with Elongation of 17.8 % | Predicted Value, A200 | |||||
19.8 % Show Material materials with Elongation of 19.8 % | Predicted Value, Transverse | |||||
20.6 % Show Material materials with Elongation of 20.6 % | Predicted Value, A50 | |||||
21.2 % Show Material materials with Elongation of 21.2 % | Predicted Value, A5 | |||||
20 °C | 20 % Show Material materials with Elongation of 20 % | normalized or normalized formed (+N) | EN 10028-3 | Sheet, Flat | ||
20 °C | 21 % Show Material materials with Elongation of 21 % | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
20 °C | 22 % Show Material materials with Elongation of 22 % | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
Hardness, Brinell | 242 [-] Show Material materials with Hardness, Brinell of 242 [-] | Predicted Value, Transverse | ||||
Poisson's ratio | 0.29 [-] Show Material materials with Poisson's ratio of 0.29 [-] | Typical for Low Carbon Steel | ||||
Reduction of area | 39.0 % Show Material materials with Reduction of area of 39.0 % | Predicted Value | ||||
43.7 % Show Material materials with Reduction of area of 43.7 % | Predicted Value, Transverse | |||||
Shear modulus | 82 GPa Show Material materials with Shear modulus of 82 GPa | Typical for Low Carbon Steel | ||||
Shear strength | 512.1 MPa Show Material materials with Shear strength of 512.1 MPa | Predicted Value | ||||
Tensile strength | 20 °C | 440 - 590 MPa Show Material materials with Tensile strength of 440 - 590 MPa | normalized or normalized formed (+N) | EN 10028-3 | Sheet, Flat | |
20 °C | 450 - 630 MPa Show Material materials with Tensile strength of 450 - 630 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
20 °C | 450 - 610 MPa Show Material materials with Tensile strength of 450 - 610 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
20 °C | 450 - 600 MPa Show Material materials with Tensile strength of 450 - 600 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
20 °C | 450 - 590 MPa Show Material materials with Tensile strength of 450 - 590 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
20 °C | 460 - 630 MPa Show Material materials with Tensile strength of 460 - 630 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
20 °C | 460 - 610 MPa Show Material materials with Tensile strength of 460 - 610 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
20 °C | 460 - 600 MPa Show Material materials with Tensile strength of 460 - 600 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
20 °C | 460 - 590 MPa Show Material materials with Tensile strength of 460 - 590 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
20 °C | 470 - 630 MPa Show Material materials with Tensile strength of 470 - 630 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
20 °C | 470 - 610 MPa Show Material materials with Tensile strength of 470 - 610 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
20 °C | 470 - 600 MPa Show Material materials with Tensile strength of 470 - 600 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
20 °C | 470 - 590 MPa Show Material materials with Tensile strength of 470 - 590 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
20 °C | 490 - 630 MPa Show Material materials with Tensile strength of 490 - 630 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
20 °C | 490 - 610 MPa Show Material materials with Tensile strength of 490 - 610 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
20 °C | 490 - 600 MPa Show Material materials with Tensile strength of 490 - 600 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
20 °C | 490 - 590 MPa Show Material materials with Tensile strength of 490 - 590 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
Yield strength | 260.5 MPa Show Material materials with Yield strength of 260.5 MPa | Predicted Value, RP1 | ||||
299.8 MPa Show Material materials with Yield strength of 299.8 MPa | Predicted Value, RP1 Transverse | |||||
365.9 MPa Show Material materials with Yield strength of 365.9 MPa | Predicted Value, Transverse | |||||
371 MPa Show Material materials with Yield strength of 371 MPa | Predicted Value, RP02 | |||||
458.4 MPa Show Material materials with Yield strength of 458.4 MPa | Predicted Value, RP02 Transverse | |||||
459.6 MPa Show Material materials with Yield strength of 459.6 MPa | Predicted Value, RP05 | |||||
464 MPa Show Material materials with Yield strength of 464 MPa | Predicted Value, RP002 | |||||
20 °C | 285 MPa Show Material materials with Yield strength of 285 MPa | normalized or normalized formed (+N) | EN 10028-3 | Sheet, Flat | ||
20 °C | 295 MPa Show Material materials with Yield strength of 295 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
20 °C | 305 MPa Show Material materials with Yield strength of 305 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
20 °C | 315 MPa Show Material materials with Yield strength of 315 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
20 °C | 335 MPa Show Material materials with Yield strength of 335 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
20 °C | 345 MPa Show Material materials with Yield strength of 345 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
20 °C | 355 MPa Show Material materials with Yield strength of 355 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat |
Thermal
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Coefficient of thermal expansion | -100 °C | 1.08e-05 1/K Show Material materials with Coefficient of thermal expansion of 1.08e-05 1/K | normalized or normalized formed (+N) | EN 10028-3 | Flat | |
20 °C | 1.19e-05 1/K Show Material materials with Coefficient of thermal expansion of 1.19e-05 1/K | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
100 °C | 1.25e-05 1/K Show Material materials with Coefficient of thermal expansion of 1.25e-05 1/K | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
200 °C | 1.3e-05 1/K Show Material materials with Coefficient of thermal expansion of 1.3e-05 1/K | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
300 °C | 1.36e-05 1/K Show Material materials with Coefficient of thermal expansion of 1.36e-05 1/K | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
400 °C | 1.41e-05 1/K Show Material materials with Coefficient of thermal expansion of 1.41e-05 1/K | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
500 °C | 1.45e-05 1/K Show Material materials with Coefficient of thermal expansion of 1.45e-05 1/K | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
600 °C | 1.49e-05 1/K Show Material materials with Coefficient of thermal expansion of 1.49e-05 1/K | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
Max service temperature | -60 °C Show Material materials with Max service temperature of -60 °C | normalized or normalized formed (+N) | EN 10028-3 | Flat | Long | |
500 °C Show Material materials with Max service temperature of 500 °C | Typical for Carbon Steel | |||||
Melting point | 1480 - 1526 °C Show Material materials with Melting point of 1480 - 1526 °C | Typical for Low Carbon Steel | ||||
Specific heat capacity | -100 °C | 423 J/(kg·K) Show Material materials with Specific heat capacity of 423 J/(kg·K) | normalized or normalized formed (+N) | EN 10028-3 | Flat | |
20 °C | 430 J/(kg·K) Show Material materials with Specific heat capacity of 430 J/(kg·K) | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
20 °C | 430 - 461 J/(kg·K) Show Material materials with Specific heat capacity of 430 - 461 J/(kg·K) | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
20 °C | 461 J/(kg·K) Show Material materials with Specific heat capacity of 461 J/(kg·K) | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
100 °C | 479 J/(kg·K) Show Material materials with Specific heat capacity of 479 J/(kg·K) | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
200 °C | 499 J/(kg·K) Show Material materials with Specific heat capacity of 499 J/(kg·K) | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
300 °C | 517 J/(kg·K) Show Material materials with Specific heat capacity of 517 J/(kg·K) | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
400 °C | 536 J/(kg·K) Show Material materials with Specific heat capacity of 536 J/(kg·K) | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
500 °C | 558 J/(kg·K) Show Material materials with Specific heat capacity of 558 J/(kg·K) | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
600 °C | 587 J/(kg·K) Show Material materials with Specific heat capacity of 587 J/(kg·K) | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
Thermal conductivity | -100 °C | 37.6 W/(m·K) Show Material materials with Thermal conductivity of 37.6 W/(m·K) | normalized or normalized formed (+N) | EN 10028-3 | Flat | |
20 °C | 42 W/(m·K) Show Material materials with Thermal conductivity of 42 W/(m·K) | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
20 °C | 42 - 42.2 W/(m·K) Show Material materials with Thermal conductivity of 42 - 42.2 W/(m·K) | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
20 °C | 42.2 W/(m·K) Show Material materials with Thermal conductivity of 42.2 W/(m·K) | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
100 °C | 43.2 W/(m·K) Show Material materials with Thermal conductivity of 43.2 W/(m·K) | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
200 °C | 42.9 W/(m·K) Show Material materials with Thermal conductivity of 42.9 W/(m·K) | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
300 °C | 41.2 W/(m·K) Show Material materials with Thermal conductivity of 41.2 W/(m·K) | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
400 °C | 39.1 W/(m·K) Show Material materials with Thermal conductivity of 39.1 W/(m·K) | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
500 °C | 36.6 W/(m·K) Show Material materials with Thermal conductivity of 36.6 W/(m·K) | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
600 °C | 34.1 W/(m·K) Show Material materials with Thermal conductivity of 34.1 W/(m·K) | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
Thermal diffusivity | -100 °C | 12.9 mm²/s Show Material materials with Thermal diffusivity of 12.9 mm²/s | normalized or normalized formed (+N) | EN 10028-3 | Flat | |
20 °C | 11.7 mm²/s Show Material materials with Thermal diffusivity of 11.7 mm²/s | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
100 °C | 11.2 mm²/s Show Material materials with Thermal diffusivity of 11.2 mm²/s | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
200 °C | 10.3 mm²/s Show Material materials with Thermal diffusivity of 10.3 mm²/s | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
300 °C | 9.4 mm²/s Show Material materials with Thermal diffusivity of 9.4 mm²/s | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
400 °C | 8.3 mm²/s Show Material materials with Thermal diffusivity of 8.3 mm²/s | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
500 °C | 7.1 mm²/s Show Material materials with Thermal diffusivity of 7.1 mm²/s | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
600 °C | 5.7 mm²/s Show Material materials with Thermal diffusivity of 5.7 mm²/s | normalized or normalized formed (+N) | EN 10028-3 | Flat |
Electrical
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Electrical conductivity | 5 S/m Show Material materials with Electrical conductivity of 5 S/m | Predicted Value | ||||
Electrical resistivity | -100 °C | 1.82e-07 Ω·m Show Material materials with Electrical resistivity of 1.82e-07 Ω·m | normalized or normalized formed (+N) | EN 10028-3 | Flat | |
20 °C | 2.47e-07 - 2.5e-07 Ω·m Show Material materials with Electrical resistivity of 2.47e-07 - 2.5e-07 Ω·m | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
20 °C | 2.47e-07 Ω·m Show Material materials with Electrical resistivity of 2.47e-07 Ω·m | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
20 °C | 2.5e-07 Ω·m Show Material materials with Electrical resistivity of 2.5e-07 Ω·m | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
100 °C | 2.96e-07 Ω·m Show Material materials with Electrical resistivity of 2.96e-07 Ω·m | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
200 °C | 3.68e-07 Ω·m Show Material materials with Electrical resistivity of 3.68e-07 Ω·m | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
300 °C | 4.55e-07 Ω·m Show Material materials with Electrical resistivity of 4.55e-07 Ω·m | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
400 °C | 5.56e-07 Ω·m Show Material materials with Electrical resistivity of 5.56e-07 Ω·m | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
500 °C | 6.75e-07 Ω·m Show Material materials with Electrical resistivity of 6.75e-07 Ω·m | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
600 °C | 8.13e-07 Ω·m Show Material materials with Electrical resistivity of 8.13e-07 Ω·m | normalized or normalized formed (+N) | EN 10028-3 | Flat |
Magnetic
Property | Value | Comment |
---|---|---|
Curie temperature | 770 °C Show Material materials with Curie temperature of 770 °C | Typical for Low Carbon Steel |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Aluminium | 0.02 % Show Material materials with Aluminium of 0.02 % | normalized or normalized formed (+N) | EN 10028-3 | Flat, Sheet |
Carbon | 0.18 % Show Material materials with Carbon of 0.18 % | normalized or normalized formed (+N) | EN 10028-3 | Flat, Sheet |
Chromium | 0.3 % Show Material materials with Chromium of 0.3 % | normalized or normalized formed (+N) | EN 10028-3 | Flat, Sheet |
Copper | 0.3 % Show Material materials with Copper of 0.3 % | normalized or normalized formed (+N) | EN 10028-3 | Flat, Sheet |
Manganese | 1.1 - 1.7 % Show Material materials with Manganese of 1.1 - 1.7 % | normalized or normalized formed (+N) | EN 10028-3 | Flat, Sheet |
Molybdenum | 0.08 % Show Material materials with Molybdenum of 0.08 % | normalized or normalized formed (+N) | EN 10028-3 | Flat, Sheet |
Nickel | 0.5 % Show Material materials with Nickel of 0.5 % | normalized or normalized formed (+N) | EN 10028-3 | Flat, Sheet |
Niobium | 0.05 % Show Material materials with Niobium of 0.05 % | normalized or normalized formed (+N) | EN 10028-3 | Flat, Sheet |
Nitrogen | 0.012 % Show Material materials with Nitrogen of 0.012 % | normalized or normalized formed (+N) | EN 10028-3 | Flat, Sheet |
Phosphorus | 0.025 % Show Material materials with Phosphorus of 0.025 % | normalized or normalized formed (+N) | EN 10028-3 | Flat, Sheet |
Silicon | 0.5 % Show Material materials with Silicon of 0.5 % | normalized or normalized formed (+N) | EN 10028-3 | Flat, Sheet |
Sulfur | 0.015 % Show Material materials with Sulfur of 0.015 % | normalized or normalized formed (+N) | EN 10028-3 | Flat, Sheet |
Titanium | 0.03 % Show Material materials with Titanium of 0.03 % | normalized or normalized formed (+N) | EN 10028-3 | Flat, Sheet |
Vanadium | 0.1 % Show Material materials with Vanadium of 0.1 % | normalized or normalized formed (+N) | EN 10028-3 | Flat, Sheet |
Technological properties
Property | ||
---|---|---|
Supplier Disclaimer | The given information is a rough description and some properties can depend on various factors such as product thickness. Please contact the supplier or refer to the related norm or standard for further information. |
Do you have a technical question or need more information about this material?
Post it as a comment below and receive answers from engineers and other community members.