Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Density | 20 °C | 7.84 g/cm³ Show Material materials with Density of 7.84 g/cm³ | normalized and stress-relieved | EN 10028-3 | Sheet |
Mechanical
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Elastic modulus | -100 °C | 217 GPa Show Material materials with Elastic modulus of 217 GPa | normalized and stress-relieved | EN 10028-3 | Sheet | |
20 °C | 200 - 212 GPa Show Material materials with Elastic modulus of 200 - 212 GPa | normalized and stress-relieved | EN 10028-3 | Sheet | ||
20 °C | 200 GPa Show Material materials with Elastic modulus of 200 GPa | normalized and stress-relieved | EN 10028-3 | Sheet | ||
20 °C | 212 GPa Show Material materials with Elastic modulus of 212 GPa | normalized and stress-relieved | EN 10028-3 | Sheet | ||
100 °C | 207 GPa Show Material materials with Elastic modulus of 207 GPa | normalized and stress-relieved | EN 10028-3 | Sheet | ||
200 °C | 199 GPa Show Material materials with Elastic modulus of 199 GPa | normalized and stress-relieved | EN 10028-3 | Sheet | ||
300 °C | 192 GPa Show Material materials with Elastic modulus of 192 GPa | normalized and stress-relieved | EN 10028-3 | Sheet | ||
400 °C | 184 GPa Show Material materials with Elastic modulus of 184 GPa | normalized and stress-relieved | EN 10028-3 | Sheet | ||
500 °C | 175 GPa Show Material materials with Elastic modulus of 175 GPa | normalized and stress-relieved | EN 10028-3 | Sheet | ||
600 °C | 164 GPa Show Material materials with Elastic modulus of 164 GPa | normalized and stress-relieved | EN 10028-3 | Sheet | ||
Poisson's ratio | 20 °C | 0.29 [-] Show Material materials with Poisson's ratio of 0.29 [-] | normalized and stress-relieved | EN 10028-3 | Sheet | |
Shear modulus | 82 GPa Show Material materials with Shear modulus of 82 GPa | Typical for Low Carbon Steel |
Thermal
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Coefficient of thermal expansion | -100 °C | 1.05e-05 1/K Show Material materials with Coefficient of thermal expansion of 1.05e-05 1/K | normalized and stress-relieved | EN 10028-3 | Sheet | |
20 °C | 1.15e-05 1/K Show Material materials with Coefficient of thermal expansion of 1.15e-05 1/K | normalized and stress-relieved | EN 10028-3 | Sheet | ||
100 °C | 1.21e-05 1/K Show Material materials with Coefficient of thermal expansion of 1.21e-05 1/K | normalized and stress-relieved | EN 10028-3 | Sheet | ||
200 °C | 1.27e-05 1/K Show Material materials with Coefficient of thermal expansion of 1.27e-05 1/K | normalized and stress-relieved | EN 10028-3 | Sheet | ||
300 °C | 1.32e-05 1/K Show Material materials with Coefficient of thermal expansion of 1.32e-05 1/K | normalized and stress-relieved | EN 10028-3 | Sheet | ||
400 °C | 1.36e-05 1/K Show Material materials with Coefficient of thermal expansion of 1.36e-05 1/K | normalized and stress-relieved | EN 10028-3 | Sheet | ||
500 °C | 1.4e-05 1/K Show Material materials with Coefficient of thermal expansion of 1.4e-05 1/K | normalized and stress-relieved | EN 10028-3 | Sheet | ||
600 °C | 1.44e-05 1/K Show Material materials with Coefficient of thermal expansion of 1.44e-05 1/K | normalized and stress-relieved | EN 10028-3 | Sheet | ||
Max service temperature | 500 °C Show Material materials with Max service temperature of 500 °C | Typical for Carbon Steel | ||||
Melting point | 1480 - 1526 °C Show Material materials with Melting point of 1480 - 1526 °C | Typical for Low Carbon Steel | ||||
Specific heat capacity | -100 °C | 423 J/(kg·K) Show Material materials with Specific heat capacity of 423 J/(kg·K) | normalized and stress-relieved | EN 10028-3 | Sheet | |
20 °C | 461 J/(kg·K) Show Material materials with Specific heat capacity of 461 J/(kg·K) | normalized and stress-relieved | EN 10028-3 | Sheet | ||
100 °C | 479 J/(kg·K) Show Material materials with Specific heat capacity of 479 J/(kg·K) | normalized and stress-relieved | EN 10028-3 | Sheet | ||
200 °C | 499 J/(kg·K) Show Material materials with Specific heat capacity of 499 J/(kg·K) | normalized and stress-relieved | EN 10028-3 | Sheet | ||
300 °C | 517 J/(kg·K) Show Material materials with Specific heat capacity of 517 J/(kg·K) | normalized and stress-relieved | EN 10028-3 | Sheet | ||
400 °C | 536 J/(kg·K) Show Material materials with Specific heat capacity of 536 J/(kg·K) | normalized and stress-relieved | EN 10028-3 | Sheet | ||
500 °C | 558 J/(kg·K) Show Material materials with Specific heat capacity of 558 J/(kg·K) | normalized and stress-relieved | EN 10028-3 | Sheet | ||
600 °C | 587 J/(kg·K) Show Material materials with Specific heat capacity of 587 J/(kg·K) | normalized and stress-relieved | EN 10028-3 | Sheet | ||
Thermal conductivity | -100 °C | 34.7 W/(m·K) Show Material materials with Thermal conductivity of 34.7 W/(m·K) | normalized and stress-relieved | EN 10028-3 | Sheet | |
20 °C | 39.7 W/(m·K) Show Material materials with Thermal conductivity of 39.7 W/(m·K) | normalized and stress-relieved | EN 10028-3 | Sheet | ||
100 °C | 40.9 W/(m·K) Show Material materials with Thermal conductivity of 40.9 W/(m·K) | normalized and stress-relieved | EN 10028-3 | Sheet | ||
200 °C | 41 W/(m·K) Show Material materials with Thermal conductivity of 41 W/(m·K) | normalized and stress-relieved | EN 10028-3 | Sheet | ||
300 °C | 39.9 W/(m·K) Show Material materials with Thermal conductivity of 39.9 W/(m·K) | normalized and stress-relieved | EN 10028-3 | Sheet | ||
400 °C | 38.2 W/(m·K) Show Material materials with Thermal conductivity of 38.2 W/(m·K) | normalized and stress-relieved | EN 10028-3 | Sheet | ||
500 °C | 36.1 W/(m·K) Show Material materials with Thermal conductivity of 36.1 W/(m·K) | normalized and stress-relieved | EN 10028-3 | Sheet | ||
600 °C | 33.8 W/(m·K) Show Material materials with Thermal conductivity of 33.8 W/(m·K) | normalized and stress-relieved | EN 10028-3 | Sheet | ||
Thermal diffusivity | -100 °C | 11.9 mm²/s Show Material materials with Thermal diffusivity of 11.9 mm²/s | normalized and stress-relieved | EN 10028-3 | Sheet | |
20 °C | 11 mm²/s Show Material materials with Thermal diffusivity of 11 mm²/s | normalized and stress-relieved | EN 10028-3 | Sheet | ||
100 °C | 10.5 mm²/s Show Material materials with Thermal diffusivity of 10.5 mm²/s | normalized and stress-relieved | EN 10028-3 | Sheet | ||
200 °C | 9.9 mm²/s Show Material materials with Thermal diffusivity of 9.9 mm²/s | normalized and stress-relieved | EN 10028-3 | Sheet | ||
300 °C | 9.1 mm²/s Show Material materials with Thermal diffusivity of 9.1 mm²/s | normalized and stress-relieved | EN 10028-3 | Sheet | ||
400 °C | 8.1 mm²/s Show Material materials with Thermal diffusivity of 8.1 mm²/s | normalized and stress-relieved | EN 10028-3 | Sheet | ||
500 °C | 6.9 mm²/s Show Material materials with Thermal diffusivity of 6.9 mm²/s | normalized and stress-relieved | EN 10028-3 | Sheet | ||
600 °C | 5.7 mm²/s Show Material materials with Thermal diffusivity of 5.7 mm²/s | normalized and stress-relieved | EN 10028-3 | Sheet |
Electrical
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Electrical resistivity | -100 °C | 1.97e-07 Ω·m Show Material materials with Electrical resistivity of 1.97e-07 Ω·m | normalized and stress-relieved | EN 10028-3 | Sheet |
20 °C | 2.62e-07 Ω·m Show Material materials with Electrical resistivity of 2.62e-07 Ω·m | normalized and stress-relieved | EN 10028-3 | Sheet | |
100 °C | 3.13e-07 Ω·m Show Material materials with Electrical resistivity of 3.13e-07 Ω·m | normalized and stress-relieved | EN 10028-3 | Sheet | |
200 °C | 3.85e-07 Ω·m Show Material materials with Electrical resistivity of 3.85e-07 Ω·m | normalized and stress-relieved | EN 10028-3 | Sheet | |
300 °C | 4.7e-07 Ω·m Show Material materials with Electrical resistivity of 4.7e-07 Ω·m | normalized and stress-relieved | EN 10028-3 | Sheet | |
400 °C | 5.69e-07 Ω·m Show Material materials with Electrical resistivity of 5.69e-07 Ω·m | normalized and stress-relieved | EN 10028-3 | Sheet | |
500 °C | 6.85e-07 Ω·m Show Material materials with Electrical resistivity of 6.85e-07 Ω·m | normalized and stress-relieved | EN 10028-3 | Sheet | |
600 °C | 8.2e-07 Ω·m Show Material materials with Electrical resistivity of 8.2e-07 Ω·m | normalized and stress-relieved | EN 10028-3 | Sheet |
Magnetic
Property | Value | Comment |
---|---|---|
Curie temperature | 770 °C Show Material materials with Curie temperature of 770 °C | Typical for Low Carbon Steel |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Aluminium | 0.005 % Show Material materials with Aluminium of 0.005 % | normalized and stress-relieved | EN 10028-3 | Sheet |
Carbon | 0.2 Show Material materials with Carbon of 0.2 | normalized and stress-relieved | EN 10028-3 | Sheet |
Chromium | 0.3 Show Material materials with Chromium of 0.3 | normalized and stress-relieved | EN 10028-3 | Sheet |
Copper | 0.2 Show Material materials with Copper of 0.2 | normalized and stress-relieved | EN 10028-3 | Sheet |
Manganese | 1 - 1.7 % Show Material materials with Manganese of 1 - 1.7 % | normalized and stress-relieved | EN 10028-3 | Sheet |
Molybdenum | 0.1 Show Material materials with Molybdenum of 0.1 | normalized and stress-relieved | EN 10028-3 | Sheet |
Nickel | 0.4 Show Material materials with Nickel of 0.4 | normalized and stress-relieved | EN 10028-3 | Sheet |
Nitrogen | 0.025 Show Material materials with Nitrogen of 0.025 | normalized and stress-relieved | EN 10028-3 | Sheet |
Phosphorus | 0.03 Show Material materials with Phosphorus of 0.03 | normalized and stress-relieved | EN 10028-3 | Sheet |
Silicon | 0.1 - 0.6 % Show Material materials with Silicon of 0.1 - 0.6 % | normalized and stress-relieved | EN 10028-3 | Sheet |
Sulfur | 0.02 Show Material materials with Sulfur of 0.02 | normalized and stress-relieved | EN 10028-3 | Sheet |
Vanadium | 0.1 - 0.2 % Show Material materials with Vanadium of 0.1 - 0.2 % | normalized and stress-relieved | EN 10028-3 | Sheet |
Do you have a technical question or need more information about this material?
Post it as a comment below and receive answers from engineers and other community members.